Artificial diamond directional etching method
By using a mixed etching agent of ceramic powder, potassium perchlorate and copper oxide to perform surface directional etching of artificial diamond (111), the problem of indiscriminate etching caused by oxide catalysts in the prior art is solved, and efficient directional etching of diamonds is achieved The corrosion enhances the holding power and service life of the tool.
Patent Information
- Application Number
- CN202411210723.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
AI Technical Summary
Existing diamond etching methods use oxide catalysts to cause indiscriminate etching, resulting in thermal damage and reduced strength of diamonds, which cannot meet industrial needs.
Using a mixed etchant of ceramic micropowder, potassium perchlorate and copper oxide, artificial diamond (111) surface directional etching is achieved through muffle furnace heat treatment, controlling the etching temperature and time, and enhancing the holding force of the tool matrix on diamond particles.
Directed etching of artificial diamond (111) surfaces is achieved, reducing thermal damage, extending tool service life, improving tool sharpness, and reducing costs and environmental pollution.
Smart Images

Figure CN119038544A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of superhard material functionalization and relates to a method for directional etching of artificial diamond. Background Art
[0002] Artificial diamond has excellent physical and chemical properties such as strength, hardness, wear resistance, thermal conductivity, chemical stability, etc., and is widely used in industrial cutting, grinding, drilling, optics, electronics and other fields. my country is the world's largest producer of artificial diamonds, and its output has ranked first in the world for many years. Diamond has the characteristics of smooth surface and difficult wetting, which makes its interface bonding ability with the matrix poor, which is not conducive to the binding agent's holding it. There are often problems such as the binding agent is not firmly bonded, causing it to fall off prematurely, thus restricting the performance of its performance advantages.
[0003] Although my country's production of artificial diamonds has ranked first in the world, it cannot be ignored that the market share of high-end diamond products is far lower than the market share of diamond production. The performance of many artificial diamond products cannot meet industrial needs. The performance characteristics of artificial diamond products with different types of binders are quite different. Holding force is a common factor affecting the performance of all types of products. Only with appropriate holding force can artificial diamond products with excellent performance be obtained. The holding force of the binder on artificial diamond is mainly composed of mechanical interlocking force and interface bonding force between the binder and the artificial diamond interface. Changing the surface state of artificial diamond by etching to increase surface roughness and then forming an anchoring bond with the binder is one of the main ways to improve the holding force of artificial diamond tool products. Artificial diamond surface etching technology has great practical significance for improving the performance of artificial diamond products and their industrial applications. At the same time, since artificial diamonds also have broad application space in the fields of semiconductor device manufacturing and thermal management materials, but the disadvantage of artificial diamonds being difficult to process restricts the full play of their excellent properties, the research on artificial diamond single crystal surface etching technology is also helpful to promote the application of artificial diamonds in the field of functional materials.
[0004] Solid phase etching of diamond is the reverse process of diamond synthesis process, which mainly utilizes the fact that diamond is in a thermodynamically unstable state under high temperature and low pressure conditions. Existing diamond etching methods use diamond graphitizing elements such as Fe, Ni, Co, Mn and their oxides for etching. Since these metals are mainly diamond synthesis catalysts, according to the carbon phase diagram, high temperature and high pressure are used as catalysts for diamond synthesis. Under high temperature and low pressure environment, their single metals will promote diamond graphitization, while their oxides as catalysts will indiscriminately etch the diamond (111) plane and (100) crystal plane. Due to the different surface energies and atomic densities of different crystal planes of diamond, the existing etching methods have high etching temperatures and large etching degrees of different crystal planes, which cause thermal damage to diamond and reduce strength, affecting the performance of diamond. Summary of the invention
[0005] The purpose of the present invention is to provide a method for directional etching of artificial diamond, which solves the problem in the prior art that oxides used as catalysts will indiscriminately etch diamond crystal surfaces.
[0006] The technical solution adopted by the present invention is a method for directional etching of artificial diamond, comprising the following steps:
[0007] Step 1: prepare an etchant, which is a mixture of ceramic micropowder, potassium perchlorate and copper oxide; wet the artificial diamond, mix the wetting agent and the artificial diamond and stir for 5-10 minutes;
[0008] Step 2: mixing the etchant with the wetted artificial diamond to obtain a powder;
[0009] Step 3: Spread the powder evenly on a high temperature resistant tray with a thickness of 40-60mm and let it stand for 48-96h;
[0010] Step 4: placing the high temperature resistant tray into a muffle furnace for etching heat treatment, and after the treatment is completed, the system is naturally cooled to room temperature to obtain the material;
[0011] Step 5: Clean the material to remove surface residues and dry the material to obtain artificial diamond with a directionally etched (111) surface.
[0012] The present invention is also characterized in that:
[0013] The ceramic powder is one or both of silicon dioxide powder and aluminum oxide powder.
[0014] The mass ratio of copper oxide to potassium perchlorate is 1:(0.2-0.4), and the mass ratio of copper oxide to ceramic micropowder is 1:(2-4).
[0015] The preparation method of the etching agent is to place ceramic powder, potassium perchlorate and copper oxide in a mixer at the same time, and the mixing time is 40-60 minutes, wherein the mass ratio of copper oxide to potassium perchlorate is 1:(0.2-0.4), and the mass ratio of copper oxide to ceramic powder is 1:(2-4).
[0016] The particle size of the ceramic micro powder is 10-200 μm; the particle size of potassium perchlorate is 1-20 μm; the particle size of copper oxide is 5-50 μm, and the purity of the ceramic micro powder, potassium perchlorate and copper oxide is 99.9%.
[0017] The wetting agent is one or both of alcohol and ethylene glycol.
[0018] Specifically, the wetting is to take artificial diamond. When the particle size of artificial diamond is 120 / 140 or finer, the volume ratio of the mass of artificial diamond to the wetting agent is 1: (0.06-0.09) g / ml; when the particle size of artificial diamond is 100 / 120-60 / 70, the volume ratio of the mass of artificial diamond to the wetting agent is 1: (0.05-0.08) g / ml; when the particle size of artificial diamond is 50 / 60 or coarse, the volume ratio of the mass of artificial diamond to the wetting agent is 1: (0.04-0.07) g / ml.
[0019] Specifically, when the particle size of the artificial diamond is 120 / 140 or finer, the mass ratio of the artificial diamond to the etchant is 1:(1-1.2); when the particle size of the artificial diamond is 100 / 120-60 / 70, the mass ratio of the artificial diamond to the etchant is 1:(0.8-1); when the particle size of the artificial diamond is 50 / 60 or coarse, the mass ratio of the artificial diamond to the etchant is 1:(0.6-0.8).
[0020] The mixing process specifically includes placing a certain mass ratio of the etchant and the artificial diamond in a mixer, and the mixing time is 10-15 minutes.
[0021] The treatment in the muffle furnace is specifically to raise the temperature of the muffle furnace stepwise to 500-700°C, keep the temperature for 20-50 minutes, and naturally cool to room temperature after the treatment.
[0022] The beneficial effects of the present invention are:
[0023] 1. The etchant of the present invention can realize directional etching of artificial diamond. The etching effect can be effectively controlled by changing the etchant ratio, etching temperature and holding time, thereby realizing effective control of the degree of directional etching of the (111) surface and enhancing the holding force of the tool substrate on the artificial diamond particles, thereby achieving the purpose of extending the service life of the tool and increasing the sharpness of the tool.
[0024] 2. Compared with the existing etching methods, the directional etching of the (111) surface of the present invention has a smaller etching area, which effectively avoids a series of problems caused by excessive reduction in the strength of artificial diamond.
[0025] 3. The etching temperature of copper oxide is 100-200℃ lower than that of metal iron, nickel, cobalt and their oxides, which can effectively reduce the thermal damage caused by roughening the surface of artificial diamond;
[0026] 4. The etchant of the present invention is a mixture of ceramic micropowder, potassium perchlorate and copper oxide. The etchant can be reused, which reduces costs and acid treatment pollution in traditional etching methods and protects the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1Schematic diagram of the unetched artificial diamond surface;
[0028] Figure 2 This is a schematic diagram of the artificial diamond (111) surface after etching in Example 1 of the present invention;
[0029] Figure 3 Schematic diagram of etching the (111) and (100) surfaces of artificial diamond in the prior art. DETAILED DESCRIPTION
[0030] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] like Figure 1-3 The present invention provides a technical solution: a method for directional etching of artificial diamond, comprising the following steps:
[0032] Step 1: prepare an etchant, which is a mixture of ceramic micropowder, potassium perchlorate and copper oxide; wet the artificial diamond, mix the wetting agent and the artificial diamond and stir for 5-10 minutes; the ceramic micropowder is one or two of silicon dioxide powder and aluminum oxide powder, and the preparation method of the etchant is to put a certain mass ratio of ceramic micropowder, potassium perchlorate and copper oxide in a mixer at the same time, and mix for 40-60 minutes, the particle size of the ceramic micropowder is 10-200μm; the particle size of potassium perchlorate is 1-20μm, the particle size of copper oxide is 5-50μm, the purity of ceramic micropowder, potassium perchlorate and copper oxide is 99.9%, and the mass ratio of copper oxide to potassium perchlorate is 1:(0.2-0.4), the mass ratio of copper oxide to ceramic powder is 1:(2-4), the wetting agent is one or both of alcohol and ethylene glycol, and the wetting operation is specifically to take artificial diamond, when the particle size of artificial diamond is 120 / 140 or finer, the volume ratio of the mass of artificial diamond to the wetting agent is 1:(0.06-0.09) g / ml; when the particle size of artificial diamond is 100 / 120-60 / 70, the volume ratio of the mass of artificial diamond to the wetting agent is 1:(0.05-0.08) g / ml; when the particle size of artificial diamond is 50 / 60 or coarse, the volume ratio of the mass of artificial diamond to the wetting agent is 1:(0.04-0.07) g / ml.
[0033] Step 2: Mixing the etchant with the wetted artificial diamond to obtain a powder, wherein the mixing is specifically when the artificial diamond particle size is 120 / 140 or finer, the mass ratio of the artificial diamond to the etchant is 1:(1-1.2); when the artificial diamond particle size is 100 / 120-60 / 70, the mass ratio of the artificial diamond to the etchant is 1:(0.8-1); when the artificial diamond particle size is 50 / 60 or coarse, the mass ratio of the artificial diamond to the etchant is 1:(0.6-0.8), and the mixing is specifically placing ceramic powder, potassium perchlorate and copper oxide in a mixer at the same time, and the mixing time is 40-60 minutes, wherein the mass ratio of copper oxide to potassium perchlorate is 1:(0.2-0.4), and the mass ratio of copper oxide to ceramic powder is 1:(2-4).
[0034] Step 3: Spread the powder evenly on a high temperature resistant tray with a thickness of 40-60mm and let it stand for 48-96h;
[0035] Step 4: placing the high temperature resistant tray into a muffle furnace for etching heat treatment, and after the treatment is completed, the system is naturally cooled to room temperature to obtain the material, and the treatment in the muffle furnace is specifically to heat the muffle furnace stepwise to 500-700°C, keep warm for 1-30 minutes, and naturally cool to room temperature after the treatment is completed; wherein the step-by-step heating is specifically as follows: the first stage is to heat up to 40°C for 5 minutes, and keep warm at 40°C for 10 minutes; the second stage is to heat up to 120°C for 10 minutes, and keep warm at 120°C for 5 minutes; the third stage is to heat up to 550°C for 30 minutes, and keep warm at 550°C for 5 minutes; the fourth stage is to heat up to 500-700°C for 20 minutes, and keep warm at 500-700°C for 20-50 minutes;
[0036] Step 5: Clean the material to remove surface residues and dry the material to obtain artificial diamond with a directionally etched (111) surface.
[0037] Example 1
[0038] Select silica powder with a particle size of 10 μm, potassium perchlorate with a particle size of 1 μm, and copper oxide with a particle size of 5 μm to prepare an etchant, wherein the mass ratio of copper oxide to potassium perchlorate is 1:0.2, and the mass ratio of copper oxide to silica powder is 1:0.4. Place the mixture in a mixer for mixing. The mixer rotates at a speed of 30 r / min and the mixing time is 40 min. After mixing, take it out for use.
[0039] In addition, artificial diamond with the brand of ZND2040 and the particle size of 140 / 170 was selected, and 2000g of artificial diamond was weighed, and the artificial diamond was mixed with 120ml of alcohol for 5min to fully soak the surface of the artificial diamond. The fully soaked artificial diamond was mixed with 2000g of the etchant, and the stirring mixing time was 15min. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 40mm, and allowed to stand for 96h. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were heating to 40℃ for 5min and keeping warm for 10min; heating to 120℃ for 10min and keeping warm for 5min; heating to 550℃ for 30min and keeping warm for 5min; heating to 655℃ for 20min and keeping warm for 50min. After the treatment was completed, it was naturally cooled. After the material was cooled to room temperature, the surface residue was cleaned to remove it, and the material was dried to obtain the artificial diamond 1 with the (111) surface etched in a directional manner.
[0040] Example 2
[0041] Silica powder with a particle size of 10 μm was selected as ceramic powder, potassium perchlorate with a particle size of 1 μm, and copper oxide with a particle size of 5 μm was selected to prepare an etchant, wherein the mass ratio of copper oxide to potassium perchlorate was 1:0.2, and the mass ratio of copper oxide to ceramic powder was 1:0.4. The mixture was placed in a mixer for mixing. The speed of the mixer was 30 r / min, and the mixing time was 40 min. After mixing, the mixture was taken out for use.
[0042] In addition, artificial diamond with the brand of ZND2040 and the particle size of 140 / 170 was selected, and 2000g of artificial diamond was weighed, and the artificial diamond was mixed with 180ml of wetting agent for 8min, wherein the wetting agent was a mixture of alcohol and ethylene glycol in a ratio of 1:1, so that the surface of the artificial diamond was fully soaked. The fully soaked artificial diamond was mixed with 2400g of the etchant, and the stirring mixing time was 15min. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 40mm, and allowed to stand for 96h. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were heating to 40℃ for 5min and keeping warm for 10min; heating to 120℃ for 10min and keeping warm for 5min; heating to 550℃ for 30min and keeping warm for 5min; heating to 695℃ for 20min and keeping warm for 50min. After the treatment is completed, the material is naturally cooled. After the material is cooled to room temperature, the surface residue is cleaned to remove the surface residue, and the material is dried to obtain the artificial diamond 2 with a directionally etched (111) surface.
[0043] Example 3
[0044] Silica powder with a particle size of 10 μm was selected as ceramic powder, potassium perchlorate with a particle size of 1 μm, and copper oxide with a particle size of 5 μm was selected to prepare an etchant, wherein the mass ratio of copper oxide to potassium perchlorate was 1:0.3, and the mass ratio of copper oxide to ceramic powder was 1:3.5. The mixture was placed in a mixer for mixing. The speed of the mixer was 30 r / min, and the mixing time was 40 min. After mixing, the mixture was taken out for use.
[0045] In addition, artificial diamond with the brand of ZND2040 and the particle size of 120 / 140 was selected, and 2000g of artificial diamond was weighed, and the artificial diamond was mixed with 160ml of alcohol for 10min to fully soak the surface of the artificial diamond. The fully soaked artificial diamond was mixed with 2200g of the etchant, and the stirring mixing time was 15min. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 40mm, and allowed to stand for 96h. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were heating to 40℃ for 5min and keeping warm for 10min; heating to 120℃ for 10min and keeping warm for 5min; heating to 550℃ for 30min and keeping warm for 5min; heating to 500℃ for 20min and keeping warm for 50min. After the treatment was completed, it was naturally cooled. After the material was cooled to room temperature, the surface residue was cleaned to remove it, and the material was dried to obtain the artificial diamond 3 with the (111) surface etched in a directional manner.
[0046] Example 4
[0047] Silica powder with a particle size of 60 μm was selected as ceramic powder, potassium perchlorate with a particle size of 15 μm, and copper oxide with a particle size of 25 μm was selected to prepare an etchant, wherein the mass ratio of copper oxide to potassium perchlorate was 1:0.25, and the mass ratio of copper oxide to ceramic powder was 1:4. The mixture was placed in a mixer for mixing. The speed of the mixer was 30 r / min, and the mixing time was 45 min. After mixing, the mixture was taken out for use.
[0048] In addition, artificial diamond with the brand ZND2040 and the particle size of 100 / 120 was selected, and 2000g of artificial diamond was weighed. The artificial diamond was mixed with 100ml of alcohol for 10 minutes to fully wet the surface of the artificial diamond. The fully wetted artificial diamond was mixed with 1600g of the etchant, and the stirring mixing time was 15 minutes. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 40mm, and allowed to stand for 90 hours. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were heating to 40°C for 5 minutes and keeping warm for 10 minutes; heating to 120°C for 10 minutes and keeping warm for 5 minutes; heating to 550°C for 30 minutes and keeping warm for 5 minutes; heating to 680°C for 20 minutes and keeping warm for 50 minutes. After the treatment was completed, it was naturally cooled. After the material was cooled to room temperature, the surface residue was cleaned to remove it, and the material was dried to obtain the artificial diamond 4 with the (111) surface etched in a directional manner.
[0049] Example 5
[0050] Silica powder with a particle size of 60 μm was selected as ceramic powder, potassium perchlorate with a particle size of 15 μm, and copper oxide with a particle size of 25 μm was selected to prepare an etchant, wherein the mass ratio of copper oxide to potassium perchlorate was 1:0.25, and the mass ratio of copper oxide to ceramic powder was 1:4. The mixture was placed in a mixer for mixing. The speed of the mixer was 30 r / min, and the mixing time was 45 min. After mixing, the mixture was taken out for use.
[0051] In addition, artificial diamond with a grade of ZND2040 and a particle size of 80 / 100 was selected, and 2000g of artificial diamond was weighed. The artificial diamond was mixed with 140ml of alcohol for 7 minutes to fully wet the surface of the artificial diamond. The fully wetted artificial diamond was mixed with 1800g of an etchant, and the stirring mixing time was 15 minutes. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 45mm, and allowed to stand for 55 hours. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were heating to 40°C for 5 minutes and keeping warm for 10 minutes; heating to 120°C for 10 minutes and keeping warm for 5 minutes; heating to 550°C for 30 minutes and keeping warm for 5 minutes; heating to 680°C for 20 minutes and keeping warm for 50 minutes. After the treatment was completed, it was naturally cooled. After the material was cooled to room temperature, the surface residue was cleaned to remove it, and the material was dried to obtain the artificial diamond 5 with a directionally etched (111) surface.
[0052] Example 6
[0053] Aluminum oxide powder and silicon dioxide powder with a particle size of 100 μm were selected as ceramic micropowders, potassium perchlorate of 5 μm, and copper oxide of 20 μm were used to prepare the etching agent, wherein the mass ratio of aluminum oxide powder to silicon dioxide powder was 1:1, the mass ratio of copper oxide to potassium perchlorate was 1:0.2, and the mass ratio of copper oxide to ceramic micropowder was 1:2. The mixture was placed in a mixer for mixing. The speed of the mixer was 30 r / min, the mixing time was 50 min, and the mixture was taken out for use after the mixing was completed.
[0054] In addition, artificial diamond with a grade of ZND2140 and a particle size of 60 / 70 was selected, and 2000g of artificial diamond was weighed, and the artificial diamond was mixed with 160ml of alcohol for 8 minutes to fully soak the surface of the artificial diamond. The fully soaked artificial diamond was mixed with 2000g of the etchant, and the stirring mixing time was 10 minutes. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 60mm, and allowed to stand for 48 hours. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were: heating to 40°C for 5 minutes, and keeping warm for 10 minutes; heating to 120°C for 10 minutes, and keeping warm for 5 minutes; heating to 550°C for 30 minutes, and keeping warm for 5 minutes; heating to 700°C for 20 minutes, and keeping warm for 30 minutes; after the treatment was completed, it was naturally cooled, and after the material was cooled to room temperature, the surface residue was cleaned to remove, and the material was dried to obtain the artificial diamond 6 with a directionally etched (111) surface.
[0055] Example 7
[0056] Aluminum oxide powder with a particle size of 100 μm was selected as ceramic powder, potassium perchlorate with a particle size of 5 μm, and copper oxide with a particle size of 20 μm was selected to prepare an etchant, wherein the mass ratio of copper oxide to potassium perchlorate was 1:0.2, and the mass ratio of copper oxide to ceramic powder was 1:2. The mixture was placed in a mixer for mixing. The speed of the mixer was 30 r / min, and the mixing time was 50 min. After mixing, the mixture was taken out for use.
[0057] In addition, artificial diamond with a grade of ZND2140 and a particle size of 50 / 60 was selected, and 2000g of artificial diamond was weighed, and the artificial diamond was mixed with 140ml of alcohol for 5 minutes to fully soak the surface of the artificial diamond. The fully soaked artificial diamond was mixed with 1600g of an etchant, and the stirring mixing time was 10 minutes. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 60mm, and allowed to stand for 48 hours. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were: heating to 40°C for 5 minutes, and keeping warm for 10 minutes; heating to 120°C for 10 minutes, and keeping warm for 5 minutes; heating to 550°C for 30 minutes, and keeping warm for 5 minutes; heating to 700°C for 20 minutes, and keeping warm for 30 minutes; after the treatment was completed, it was naturally cooled, and after the material was cooled to room temperature, the surface residue was cleaned to remove, and the material was dried to obtain the artificial diamond 7 with a directionally etched (111) surface.
[0058] Example 8
[0059] Aluminum oxide powder with a particle size of 160 μm was selected as ceramic powder, potassium perchlorate with a particle size of 10 μm, and copper oxide with a particle size of 40 μm was selected to prepare an etchant, wherein the mass ratio of copper oxide to potassium perchlorate was 1:0.4, and the mass ratio of copper oxide to ceramic powder was 1:4. The mixture was placed in a mixer for mixing. The speed of the mixer was 30 r / min, and the mixing time was 60 min. After mixing, the mixture was taken out for use.
[0060] In addition, artificial diamond with a grade of ZND2140 and a particle size of 45 / 50 was selected, and 2000g of artificial diamond was weighed, and the artificial diamond was mixed with 120ml of ethylene glycol for 6 minutes to fully wet the surface of the artificial diamond. The fully wetted artificial diamond was mixed with 1400g of an etchant, and the stirring mixing time was 12 minutes. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 50mm, and allowed to stand for 58 hours. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were: heating to 40°C for 5 minutes, and keeping warm for 10 minutes; heating to 120°C for 10 minutes, and keeping warm for 5 minutes; heating to 550°C for 30 minutes, and keeping warm for 5 minutes; heating to 600°C for 20 minutes, and keeping warm for 40 minutes; after the treatment was completed, it was naturally cooled, and after the material was cooled to room temperature, the surface residue was cleaned to remove, and the material was dried to obtain the artificial diamond 8 with a directionally etched (111) surface.
[0061] Example 9
[0062] A mixture of 200 μm aluminum oxide powder and 200 μm silicon dioxide powder in a 1:1 ratio was selected as ceramic micropowder, 20 μm potassium perchlorate, and 50 μm copper oxide were used to prepare an etchant, wherein the mass ratio of copper oxide to potassium perchlorate was 1:0.2, and the mass ratio of copper oxide to ceramic micropowder was 1:2.5. The mixture was placed in a mixer for mixing. The mixer speed was 30 r / min, the mixing time was 50 min, and the mixture was taken out for use after mixing was completed.
[0063] In addition, artificial diamond with a grade of ZND2240 and a particle size of 35 / 40 was selected, and 2000g of artificial diamond was weighed, and the artificial diamond was mixed with 80ml of ethylene glycol for 9 minutes to fully wet the surface of the artificial diamond. The fully wetted artificial diamond was mixed with 1200g of an etchant, and the stirring mixing time was 10 minutes. The fully mixed powder was evenly placed in a high-temperature resistant ceramic tray, with a flat thickness of 50mm, and allowed to stand for 68 hours. After standing, the high-temperature resistant ceramic tray was placed in a muffle furnace for heating. The specific heating conditions were: heating to 40°C for 5 minutes, and keeping warm for 10 minutes; heating to 120°C for 10 minutes, and keeping warm for 5 minutes; heating to 550°C for 30 minutes, and keeping warm for 5 minutes; heating to 700°C for 20 minutes, and keeping warm for 20 minutes; after the treatment was completed, it was naturally cooled, and after the material was cooled to room temperature, the surface residue was cleaned to remove, and the material was dried to obtain the artificial diamond 9 with a directionally etched (111) surface.
[0064] In the directional etching method of artificial diamond provided by the present invention, after fully wetting the surface of artificial diamond, an etchant is mixed to make the surface adhere to the etchant; copper oxide plays a catalytic reduction role, under which condition, directional etching of the artificial diamond (111) surface can be achieved; potassium perchlorate plays an oxidizing role as an oxygen supply agent; ceramic micropowder can effectively increase the porosity of the material and avoid the full contact of the surface of artificial diamond with the generated oxygen, thereby changing the etching surface state.
[0065] Since artificial diamond is composed of carbon, 3Hybrid crystal material, the surface carbon atoms of which are chemically adsorbed with hydrogen atoms, makes the surface atoms of artificial diamond crystal very stable and chemically inert. Copper oxide is a weak metal oxide. Under heating and catalytic conditions, copper oxide has a good chemical desorption ability for the surface atoms of artificial diamond crystal, so it can open the carbon dangling bonds of artificial diamond crystal, making it metastable; copper oxide and artificial diamond crystal carbon atoms will undergo oxidation and reduction reactions, and the gas generated by the oxidation of carbon atoms will be discharged, while the metal copper generated by the replacement of artificial diamond carbon atoms will neither catalyze the graphitization of artificial diamond carbon atoms nor cause the physical diffusion of artificial diamond carbon atoms. The surface energy of artificial diamond (111) crystal plane is lower than that of (100) crystal plane. In a unit area, more dangling bonds on the (111) plane are saturated with hydrogen atoms. The (111) plane enhances the adsorption capacity of copper oxide and realizes the directional etching of the (111) plane. The method enhances the holding force between the artificial diamond tool matrix and the artificial diamond particles by mixing non-carburized element copper oxide of specific particle size in a specific proportion and subjecting it to high temperature treatment, thereby achieving the purpose of improving the cutting efficiency and service life of the tool.
Claims
1. A method for directional etching of artificial diamond, characterized in that: The following steps are involved: Step 1: preparing an etchant, which is a mixture of ceramic micropowder, potassium perchlorate and copper oxide; wetting the artificial diamond, mixing the wetting agent and the artificial diamond and stirring for 5-10 minutes; Step 2: mixing the etchant with the wetted artificial diamond to obtain a powder; Step 3: evenly spread the powder on a high temperature resistant tray and let it stand, with a thickness of 40-60 mm and a standing time of 48-96 hours; Step 4: placing the high temperature resistant tray into a muffle furnace for etching heat treatment, and after the treatment is completed, the system is naturally cooled to room temperature to obtain a material; Step 5: Clean the material to remove surface residues, and dry the material to obtain directionally etched artificial diamond.
2. The method for directional etching of artificial diamond according to claim 1, characterized in that: The ceramic powder is one or both of silicon dioxide powder and aluminum oxide powder.
3. The method for directional etching of artificial diamond according to claim 1, characterized in that: The mass ratio of the copper oxide to potassium perchlorate is 1:(0.2-0.4), and the mass ratio of the copper oxide to the ceramic powder is 1:(2-4).
4. The method for directional etching of artificial diamond according to claim 3, characterized in that: The preparation method of the etching agent is to place ceramic powder, potassium perchlorate and copper oxide in a mixer at the same time, and mix them for 40-60 minutes, wherein the mass ratio of copper oxide to potassium perchlorate is 1:(0.2-0.4), and the mass ratio of copper oxide to ceramic powder is 1:(2-4).
5. The method for directional etching of artificial diamond according to claim 1, characterized in that: The particle size of the ceramic powder is 10-200 μm; the particle size of the potassium perchlorate is 1-20 μm; the particle size of the copper oxide is 5-50 μm, and the purity of the ceramic powder, potassium perchlorate and copper oxide is 99.9%.
6. The method for directional etching of artificial diamond according to claim 1, characterized in that: The wetting agent is one or both of alcohol and ethylene glycol.
7. The method for directional etching of artificial diamond according to claim 1, characterized in that: The wetting is specifically to take artificial diamond. When the particle size of the artificial diamond is 120 / 140 or finer, the volume ratio of the mass of the artificial diamond to the wetting agent is 1: (0.06-0.09) g / ml; when the particle size of the artificial diamond is 100 / 120-60 / 70, the volume ratio of the mass of the artificial diamond to the wetting agent is 1: (0.05-0.08) g / ml; when the particle size of the artificial diamond is 50 / 60 or coarse, the volume ratio of the mass of the artificial diamond to the wetting agent is 1: (0.04-0.07) g / ml.
8. The method for directional etching of artificial diamond according to claim 1, characterized in that: Specifically, when the particle size of the artificial diamond is 120 / 140 or finer, the mass ratio of the artificial diamond to the etchant is 1:(1-1.2); when the particle size of the artificial diamond is 100 / 120-60 / 70, the mass ratio of the artificial diamond to the etchant is 1:(0.8-1); when the particle size of the artificial diamond is 50 / 60 or coarse, the mass ratio of the artificial diamond to the etchant is 1:(0.6-0.8).
9. The method for directional etching of artificial diamond according to claim 8, characterized in that: The mixing is specifically to place the etchant and the artificial diamond in a certain mass ratio in a mixer, and the mixing time is 10-15 minutes.
10. The method for directional etching of artificial diamond according to claim 1, characterized in that: The etching heat treatment specifically comprises stepwise heating the muffle furnace to 500-700° C., keeping the temperature for 20-50 minutes, and naturally cooling to room temperature after the treatment.
Citation Information
Patent Citations
Surface roughening treatment method of diamond
CN107473768A
High-oriented method for etching diamond (100) face
CN110540200A
Artificial diamond surface etching method
CN113716560A
Copper-diamond composite material as well as preparation method and application thereof
CN118326479A