Comprehensive utilization method of acidic wastewater in glass thinning industry
By using the recycling technology of sodium fluoride and magnesium hydroxide in the acidic wastewater treatment in the glass thinning industry, fluorosiliic acid and fluorine ions were successfully recovered, and the high energy consumption and unused acid components in the prior art were solved. The problem of this has achieved efficient and environmentally friendly wastewater treatment.
Patent Information
- Application Number
- CN202411169260.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the acidic wastewater treatment of the glass thinning industry, it is difficult for the prior art to effectively recover fluorosiliic acid and fluorine ions, and there are problems such as high energy consumption, high personnel and equipment risks, and other acid components are not used during the treatment process.
Precipitation is performed by adding sodium fluoride to fluorosilicate circulating water, followed by adding magnesium hydroxide to perform primary and secondary defluorination, combining deep defluorination and wet ball milling alkali conversion, recycling magnesium hydroxide and sodium fluoride, and finally Sodium fluoride is recovered by evaporation crystallization, and the effective recovery of fluorosilicate and fluoride ions is achieved.
It realizes efficient recycling of fluorosilicate and fluorine ions, reduces the emission of fluorine-containing waste liquid, recycles magnesium hydroxide and sodium fluoride, reduces treatment costs, and has environmentally friendly and economically friendly properties.
Smart Images

Figure CN119038782A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of waste liquid recycling and reuse in the glass thinning industry, and in particular to a comprehensive utilization method of acid waste water in the glass thinning industry. Background Art
[0002] Acid etching is the most commonly used glass thinning method. According to the composition of the acid, the etching acid is mainly divided into HF series, HF-sulfuric acid / hydrochloric acid series, HF-ammonium bifluoride / sulfuric acid / hydrochloric acid series, etc. The main principle of glass substrate thinning is to use a mixed acid solution containing HF to react with SiO2 and other metal oxides on the glass surface, so that the glass surface is peeled off, achieving the purpose of glass thinning and surface strengthening. Adding hydrochloric acid or sulfuric acid can increase the hydrogen ion concentration of the system and increase the etching rate, while ammonium bifluoride as a buffer can ensure a stable fluoride ion concentration and ensure the stability of the etching rate. As the reaction proceeds, the HF concentration in the thinning solution gradually decreases, while the fluorosilicic acid content in the system continues to increase. The increase in the fluorosilicic acid concentration not only reduces the etching ability of the system, but also causes uneven etching on the substrate surface, resulting in a decrease in product quality and an increase in etching processing time, so that the thinning solution cannot be used any more and causes waste liquid discharge.
[0003] As a hazardous waste liquid in the industry, glass thinning waste liquid is currently mainly treated by lime or limestone neutralization disposal. This method can neutralize F- and SiF6 in the waste liquid. 2- ions and pH values meet the discharge standards, but this process will produce a large amount of mixed solids containing CaSO4 and CaF2, which are hazardous wastes, increasing the cost of subsequent disposal (treatment fee ≥ 2,000 yuan / t), and wasting a large amount of unreacted HF and other useful acid raw materials in the waste liquid. A patent discloses a method for treating fluorine-containing wastewater, which does not produce any three wastes, and the concentrated acid produced during the treatment process can be reused. However, this method converts fluorine in the waste liquid into fluorine chemicals through a distillation method, which has the problems of high energy consumption and high-temperature operation, which greatly increases the danger to personnel and equipment. It also has the disadvantage of wasting the recovery and reuse of other acid components.
[0004] Therefore, how to provide a comprehensive utilization method for acidic wastewater from the glass thinning industry so that the wastewater from the glass thinning industry can be treated by the method to effectively recover fluorosilicic acid and fluoride ions in the wastewater, while recycling magnesium hydroxide and sodium fluoride during the treatment process, is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0005] In view of the problems existing in the prior art, the technical problem to be solved by the present invention is to provide a method for comprehensive utilization of acidic wastewater from the glass thinning industry, so that after the wastewater from the glass thinning industry is treated by the method, fluorosilicic acid and fluoride ions in the wastewater can be effectively recovered, the discharge of fluorine-containing waste liquid can be reduced, and the added magnesium hydroxide and sodium fluoride can be reused, which has environmentally friendly and economically friendly characteristics.
[0006] To achieve the above-mentioned purpose, the present invention provides a comprehensive utilization method of acidic wastewater in the glass thinning industry, and the comprehensive utilization method of acidic wastewater in the glass thinning industry specifically comprises: S1, precipitation: adding sodium fluoride to the fluosilicic acid circulating water, stirring to obtain a first solid-liquid mixture, and performing solid-liquid separation on the first solid-liquid mixture to obtain sodium fluosilicate and a mixed acid solution; S2, primary defluorination: adding magnesium hydroxide to the mixed acid solution obtained in S1, stirring to obtain a second solid-liquid mixture, and performing solid-liquid separation on the second solid-liquid mixture to obtain a primary defluorination liquid and a primary defluorination slag; S3, secondary defluorination: mixing the primary defluorination liquid obtained in S2 with a spray liquid, and then adding magnesium hydroxide, stirring to obtain a third solid-liquid mixture, and performing solid-liquid separation on the third solid-liquid mixture to obtain Secondary defluorination liquid and secondary defluorination slag; S4, deep defluorination: add deep defluorination agent to the secondary defluorination liquid obtained in S3, adjust pH value, and obtain deep defluorination slag and qualified tail liquid; S5, wet ball milling alkali conversion: mix the primary defluorination slag obtained in S2 and the secondary defluorination slag obtained in S3, then add sodium hydroxide, perform wet ball milling alkali conversion, obtain magnesium hydroxide and alkali conversion liquid, and then reuse the magnesium hydroxide in S2 and S3; S6, neutralization: add hydrofluoric acid to the alkali conversion liquid obtained in S5 for neutralization to obtain neutralized liquid; S7, evaporation and crystallization: evaporate and crystallize the neutralized liquid obtained in S6 to obtain sodium fluoride and crystallization mother liquor, the sodium fluoride is reused in S1, and the crystallization mother liquor is returned to S5 for wet ball milling alkali conversion.
[0007] In the first aspect, the step of adding sodium fluoride to fluorosilicic acid circulating water to obtain a first solid-liquid mixture, and subjecting the first solid-liquid mixture to solid-liquid separation to obtain sodium fluorosilicate and a mixed acid solution specifically comprises: adding sodium fluoride to fluorosilicic acid circulating water, and then stirring at a stirring speed of 200 to 400 rpm for 0.2 to 2 hours at a temperature of 20 to 40° C. to obtain a first solid-liquid mixture, and subjecting the first solid-liquid mixture to solid-liquid separation to obtain sodium fluorosilicate and a mixed acid solution; the amount of sodium fluoride used is 1.2 to 1.6 times the theoretical reaction molar ratio of the fluorosilicic acid circulating water.
[0008] In the first aspect, the step of adding magnesium hydroxide to the mixed acid solution obtained in S1, stirring to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag specifically comprises: adding magnesium hydroxide to the mixed acid solution obtained in S1, and then stirring at a stirring speed of 200 to 400 rpm for 0.2 to 2 hours at a temperature of 25 to 50° C. to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag.
[0009] In the first aspect, the amount of magnesium hydroxide used is 0.8 to 1.2 times the theoretical reaction molar ratio of the mixed acid solution.
[0010] In the first aspect, the first defluorination liquid obtained in S2 is mixed with the spray liquid, and then magnesium hydroxide is added, and stirred to obtain a third solid-liquid mixture, and the third solid-liquid mixture is subjected to solid-liquid separation to obtain a second defluorination liquid and a second defluorination slag. Specifically, the first defluorination liquid obtained in S2 is mixed with the spray liquid, and then magnesium hydroxide is added, and stirred at a temperature of 25 to 50° C. and a stirring speed of 200 to 400 rpm for 0.2 to 2 hours to obtain a third solid-liquid mixture, and the third solid-liquid mixture is subjected to solid-liquid separation to obtain a second defluorination liquid and a second defluorination slag.
[0011] In the first aspect, the volume ratio of the primary defluorination liquid to the spray liquid is 1:3 to 1:6; the amount of magnesium hydroxide added is 1.2 to 1.6 times the theoretical reaction molar ratio of the primary defluorination liquid to the spray liquid; and the spray liquid is an acidic spray liquid.
[0012] In the first aspect, the step of adding a deep defluorination agent to the secondary defluorination liquid obtained in S3 to obtain deep defluorination slag and qualified tail liquid specifically comprises: adding a deep defluorination agent to the secondary defluorination liquid obtained in S3, adjusting the pH to 5.5-8.0, stirring at a temperature of 15-35°C until no solid precipitate is generated to obtain a fourth solid-liquid mixture, and performing solid-liquid separation on the fourth solid-liquid mixture to obtain deep defluorination slag and qualified tail liquid.
[0013] In the first aspect, the added amount of the deep defluorination agent is 1.2 to 1.6 times the reaction molar ratio of fluoride ions; and the deep defluorination agent is calcium oxide.
[0014] In the first aspect, in S5, the amount of sodium hydroxide used is 1 to 2 times the theoretical reaction molar ratio of magnesium fluoride in the primary defluorination slag and the secondary defluorination slag.
[0015] In the first aspect, in S5, the ball-to-material ratio of the wet ball milling alkali rotation is 8-12, the solid-liquid ratio of the wet ball milling alkali rotation is 1-4 mL / g, the ball milling time of the wet ball milling alkali rotation is 2-4 hours, and the ball milling speed of the wet ball milling alkali rotation is 400-600 rpm.
[0016] Beneficial effects:
[0017] The invention discloses a comprehensive utilization method of acid wastewater from glass thinning industry, which is mainly used for treating the acid wastewater fluorosilicic acid circulating water from glass thinning industry. Sodium fluoride is added to the fluorosilicic acid circulating water to generate sodium fluorosilicate precipitate and mixed acid solution, and the sodium fluorosilicate is recovered. A large amount of fluoride ions in the mixed acid solution need to be removed. Magnesium hydroxide is added to the mixed acid solution for primary defluorination. The addition of magnesium hydroxide can reduce the acidity of the mixed acid solution to obtain primary defluorination slag and primary defluorination liquid. The primary defluorination slag is mainly magnesium fluoride precipitate generated by fluoride in the mixed acid and magnesium hydroxide. The remaining primary defluorination liquid is mixed with an acidic spray liquid, and the spray liquid is obtained by spraying the flue gas of the glass thinning industry. The flue gas contains some fluoride ions, so that the acidic spray liquid contains fluoride ions. The acidic spray liquid is mixed with the primary defluorination liquid for treatment, which can reduce the post-treatment cost of the flue gas treatment liquid; magnesium hydroxide is added to the mixture of the acidic spray liquid and the primary defluorination liquid to carry out secondary defluorination to obtain secondary defluorination slag and secondary defluorination liquid. The secondary defluorination slag is mainly magnesium fluoride precipitate generated by fluoride in the mixed acid and magnesium hydroxide; the primary defluorination slag and the secondary defluorination slag are collected and mixed, sodium hydroxide is added for wet ball milling alkali conversion, so that magnesium fluoride is converted into magnesium hydroxide to obtain magnesium hydroxide and sodium fluoride-containing solution, and the magnesium hydroxide is collected and reused in S2 and S3 for primary defluorination and secondary defluorination, achieving hydrogenation. The recycling of magnesium oxide reduces the consumption of chemicals and further reduces the cost of water treatment. The alkali liquid is mainly a sodium fluoride solution, which is alkaline and contains a large amount of fluoride ions, excess sodium ions and excess hydroxide ions. Hydrofluoric acid is added to the alkali liquid to consume the hydroxide ions in the alkali liquid, making the alkali liquid neutral with a pH value of 7. At this time, the main component of the alkali liquid is sodium fluoride. The alkali liquid is evaporated and crystallized, and the sodium fluoride is collected and reused in S1 to precipitate the fluorosilicic acid circulating water, thereby achieving the recycling of sodium fluoride, reducing the consumption of chemicals and further reducing the cost of water treatment. The crystallization mother liquor after evaporation and crystallization is returned to S5 to mix with the primary defluorination slag and the secondary defluorination slag. The slag is mixed and subsequently wet ball milled and alkali-converted to achieve closed-loop treatment of primary defluorination slag and secondary defluorination slag, without generating additional waste, and is environmentally friendly and economically friendly; calcium oxide is added to the secondary defluorination liquid, and the pH is adjusted, and the calcium oxide generates calcium hydroxide, which reacts with the fluoride ions in the secondary defluorination liquid to generate calcium fluoride precipitate. The main component of the deep defluorination slag is calcium fluoride. Since a large amount of fluoride-containing ions have been removed by precipitation, primary defluorination and secondary defluorination before deep defluorination, the secondary defluorination liquid contains only a small amount of fluoride-containing ions, which reduces the use of calcium oxide, thereby reducing the generation of deep defluorination slag and reducing the centralized treatment cost of deep defluorination slag, and is environmentally friendly and economically friendly;In summary, the comprehensive utilization method of acidic wastewater in the glass thinning industry of the present invention can effectively treat the fluorosilicic acid circulating water generated in the glass thinning industry, can effectively recover the fluorosilicate ions and fluoride ions in the fluorosilicic acid circulating water, and use magnesium hydroxide as a high-efficiency fluoride ion capture agent for primary defluorination and secondary defluorination. The use of magnesium hydroxide can effectively reduce the acidity in the primary defluorination liquid and the secondary defluorination liquid, the conversion of magnesium fluoride to magnesium hydroxide, and the generation of sodium fluoride in evaporation and crystallization, so as to achieve the effect of recycling magnesium hydroxide and sodium fluoride, reduce the generation of waste treatment, and have environmental friendliness and economic friendliness. ; BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 This is a process diagram of a comprehensive utilization method of acid wastewater in the glass thinning industry according to the present invention. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of this specification to clearly and completely describe the technical solutions in the embodiments of this specification. Obviously, the described embodiments are only part of the embodiments of this specification, not all of the embodiments. Based on the embodiments in this specification, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0021] Embodiment 1
[0022] like Figure 1As shown, the present embodiment 1 provides a comprehensive utilization method of acidic wastewater in the glass thinning industry, and the comprehensive utilization method of acidic wastewater in the glass thinning industry specifically includes: S1, precipitation: adding sodium fluoride to the fluosilicic acid circulating water, stirring to obtain a first solid-liquid mixture, and performing solid-liquid separation on the first solid-liquid mixture to obtain sodium fluosilicate and a mixed acid solution; S2, primary defluorination: adding magnesium hydroxide to the mixed acid solution obtained in S1, stirring to obtain a second solid-liquid mixture, and performing solid-liquid separation on the second solid-liquid mixture to obtain a primary defluorination liquid and a primary defluorination slag; S3, secondary defluorination: mixing the primary defluorination liquid obtained in S2 with the spray liquid, and then adding magnesium hydroxide, stirring to obtain a third solid-liquid mixture, and performing solid-liquid separation on the third solid-liquid mixture to obtain to secondary defluorination liquid and secondary defluorination slag; S4, deep defluorination: add deep defluorination agent to the secondary defluorination liquid obtained in S3 to obtain deep defluorination slag and qualified tail liquid; S5, wet ball milling alkali conversion: mix the primary defluorination slag obtained in S2 with the secondary defluorination slag obtained in S3, then add sodium hydroxide, perform wet ball milling alkali conversion, obtain magnesium hydroxide and alkali conversion liquid, and then reuse the magnesium hydroxide in S2 and S3; S6, neutralization: add hydrofluoric acid to the alkali conversion liquid obtained in S5 for neutralization to obtain neutralized liquid; S7, evaporation and crystallization: evaporate and crystallize the neutralized liquid obtained in S6 to obtain sodium fluoride and crystallization mother liquor, the sodium fluoride is reused in S1, and the crystallization mother liquor is returned to S5 for wet ball milling alkali conversion.
[0023] The invention discloses a comprehensive utilization method of acid wastewater in glass thinning industry, which is mainly used for treating the acid wastewater fluorosilicic acid circulating water in glass thinning industry. Sodium fluoride is added to the fluorosilicic acid circulating water to generate sodium fluorosilicate precipitate and mixed acid solution, and the sodium fluorosilicate is recovered. The mixed acid solution contains a large amount of fluoride ions that need to be removed. Magnesium hydroxide is added to the mixed acid solution for primary defluorination to obtain primary defluorination slag and primary defluorination liquid. The primary defluorination slag is mainly magnesium fluoride precipitate generated by fluoride in the mixed acid and magnesium hydroxide. The remaining primary defluorination liquid is mixed with an acidic spray liquid, and the spray liquid is the acidic spray liquid obtained by spraying the flue gas in the glass thinning industry. The flue gas contains The present invention relates to a method for removing fluorine ions from the acidic spray liquid, and removing fluorine ions from the acidic spray liquid. The acidic spray liquid is mixed with the primary defluorination liquid for treatment, which can reduce the post-treatment cost of the flue gas treatment liquid. Magnesium hydroxide is added to the mixture of the acidic spray liquid and the primary defluorination liquid for secondary defluorination to obtain secondary defluorination slag and secondary defluorination liquid. The secondary defluorination slag is mainly a magnesium fluoride precipitate generated by the fluoride in the mixed acid and magnesium hydroxide. The primary defluorination slag and the secondary defluorination slag are collected and mixed, and sodium hydroxide is added for wet ball milling and alkali conversion to convert magnesium fluoride into magnesium hydroxide to obtain magnesium hydroxide and sodium fluoride-containing solution. The magnesium hydroxide is collected and recycled to S2 and S3 for primary defluorination and secondary defluorination, thereby achieving the purpose of magnesium hydroxide. The alkali liquid is mainly a sodium fluoride solution, which is alkaline and contains a large amount of fluoride ions, excess sodium ions and excess hydroxide ions. Hydrofluoric acid is added to the alkali liquid to consume the hydroxide ions in the alkali liquid, making the alkali liquid neutral with a pH value of 7. At this time, the main component of the alkali liquid is sodium fluoride. The alkali liquid is evaporated and crystallized, and the sodium fluoride is collected and reused in S1 to precipitate the fluorosilicic acid circulating water, thereby achieving the recycling of sodium fluoride, reducing the consumption of chemicals and further reducing the water treatment cost. The crystallization mother liquor after evaporation and crystallization is returned to S5 and mixed with the primary defluorination slag and the secondary defluorination slag. The first-stage defluorination slag is mixed for subsequent wet ball milling and alkali conversion to achieve closed-loop treatment of the first-stage defluorination slag and the second-stage defluorination slag, without generating additional waste, and is environmentally friendly and economically friendly; calcium oxide is added to the second-stage defluorination liquid, and the pH is adjusted. The calcium oxide generates calcium hydroxide, which reacts with the fluoride ions in the second-stage defluorination liquid to generate calcium fluoride precipitation. The main component of the deep defluorination slag is calcium fluoride. Since a large amount of fluoride-containing ions have been removed by precipitation, first-stage defluorination and second-stage defluorination before deep defluorination, the second-stage defluorination liquid contains only a small amount of fluoride-containing ions, which greatly reduces the generation of deep defluorination slag and reduces the centralized treatment cost of deep defluorination slag, and is environmentally friendly and economically friendly;In summary, the comprehensive utilization method of acidic wastewater in the glass thinning industry of the present invention can effectively treat the fluorosilicic acid circulating water generated in the glass thinning industry, can effectively recover the fluorosilicic acid and fluoride ions in the fluorosilicic acid circulating water, and use magnesium hydroxide as a high-efficiency fluoride ion capture agent for primary and secondary defluorination. The use of magnesium hydroxide can effectively reduce the acidity in the primary and secondary defluorination liquids, the conversion of magnesium fluoride to magnesium hydroxide, and the generation of sodium fluoride in evaporation and crystallization, so as to achieve the effect of recycling magnesium hydroxide and sodium fluoride, reduce the generation of waste treatment, and have environmental friendliness and economic friendliness. ;
[0024] In some possible implementations, the step of adding sodium fluoride to fluorosilicic acid circulating water to obtain a first solid-liquid mixture, and subjecting the first solid-liquid mixture to solid-liquid separation to obtain sodium fluorosilicate and a mixed acid solution specifically comprises: adding sodium fluoride to fluorosilicic acid circulating water, and then stirring at a stirring speed of 200 to 400 rpm for 0.2 to 2 hours at a temperature of 20 to 40° C. to obtain a first solid-liquid mixture, and subjecting the first solid-liquid mixture to solid-liquid separation to obtain sodium fluorosilicate and a mixed acid solution; the amount of sodium fluoride used is 1.2 to 1.6 times the theoretical reaction molar ratio of the fluorosilicic acid circulating water.
[0025] Specifically, sodium fluoride is added to the fluosilicic acid circulating water, and the fluosilicic acid in the fluosilicic acid circulating water reacts with sodium fluoride to obtain sodium fluosilicate precipitate, and the sodium fluosilicate is separated and processed centrally to achieve the purpose of recovering fluosilicic acid; the temperature for adding sodium fluoride to react is 20 to 40°C, which is not high, and can reduce the cost caused by high-temperature operation and the danger to personnel and equipment.
[0026] In some possible implementations, the step of adding magnesium hydroxide to the mixed acid solution obtained in S1, stirring to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag specifically comprises: adding magnesium hydroxide to the mixed acid solution obtained in S1, and then stirring at a stirring speed of 200 to 400 rpm for 0.2 to 2 hours at a temperature of 25 to 50° C. to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag; and the amount of magnesium hydroxide used is 0.8 to 1.2 times the theoretical reaction molar ratio of the mixed acid solution.
[0027] Specifically, the magnesium ions in magnesium hydroxide and the fluoride ions in the mixed acid generate magnesium fluoride. The primary defluorination only removes part of the fluoride ions, and the primary defluorination liquid still contains some fluoride ions that need to be removed. Since the temperature of the primary defluorination is 25-50°C, the temperature is not high, which reduces the cost and danger to personnel and equipment caused by high-temperature operation.
[0028] In some possible implementations, the mixing of the primary defluorination liquid obtained in S2 with the spray liquid, then adding magnesium hydroxide, stirring to obtain a third solid-liquid mixture, and subjecting the third solid-liquid mixture to solid-liquid separation to obtain a secondary defluorination liquid and a secondary defluorination slag specifically includes: mixing the primary defluorination liquid obtained in S2 with the spray liquid, then adding magnesium hydroxide, stirring at a temperature of 25 to 50° C. and a stirring speed of 200 to 400 rpm for 0.2 to 2 hours to obtain a third solid-liquid mixture, and subjecting the third solid-liquid mixture to solid-liquid separation to obtain a secondary defluorination liquid and a secondary defluorination slag; the volume ratio of the primary defluorination liquid to the spray liquid is 1:3 to 1:6; the amount of magnesium hydroxide added is 1.2 to 1.6 times the theoretical reaction molar ratio of the primary defluorination liquid to the spray liquid; and the spray liquid is an acidic spray liquid.
[0029] Specifically, in the secondary defluorination, the spray liquid is a flue gas treatment waste liquid obtained after spraying the flue gas generated in the glass thinning industry. It is an acidic spray liquid. The flue gas contains fluoride ions. The acidic spray liquid containing fluoride ions is mixed with the primary defluorination liquid, and magnesium hydroxide is added to generate magnesium fluoride precipitate, which removes most of the fluoride ions and saves the cost of post-treatment of the flue gas treatment waste liquid. At the same time, the temperature of the secondary defluorination is 25-50°C, which is not high, reducing the cost of high-temperature operation and the danger to personnel and equipment.
[0030] In some possible implementations, the adding of a deep defluorinating agent to the secondary defluorinating liquid obtained in S3 to obtain a deep defluorinating slag and a qualified tail liquid specifically comprises: adding a deep defluorinating agent to the secondary defluorinating liquid obtained in S3, adjusting the pH to 5.5-8.0, stirring at a temperature of 15-35°C until no solid precipitate is generated to obtain a fourth solid-liquid mixture, and performing solid-liquid separation on the fourth solid-liquid mixture to obtain a deep defluorinating slag and a qualified tail liquid; the amount of the deep defluorinating agent added is 1.2-1.6 times the reaction molar ratio of fluoride ions; the deep defluorinating agent is calcium oxide.
[0031] Specifically, the secondary defluorination liquid contains a small amount of fluoride ions. Calcium oxide is added to the secondary defluorination liquid, and then the pH value is adjusted to 5.5-8.0 for deep defluorination. The time for deep defluorination is generally 2-6 hours. Adjusting the pH value to 5.5-8.0 can promote the conversion of calcium oxide into calcium hydroxide, promote the formation of calcium fluoride precipitation by calcium ions and fluoride ions, increase the fluoride ion removal rate, and further reduce the fluoride ion content in the qualified tail liquid. The temperature of the secondary defluorination is 15-35°C, which is not high, reducing the cost and danger to personnel and equipment caused by high-temperature operation.
[0032] In some possible implementations, in S5, the amount of sodium hydroxide used is 1 to 2 times the theoretical reaction molar ratio of magnesium fluoride in the primary defluorination slag and the secondary defluorination slag; in S5, the ball-to-material ratio of the wet ball milling alkali conversion is 8 to 12, the solid-liquid ratio of the wet ball milling alkali conversion is 1 to 4 mL / g, the ball milling time of the wet ball milling alkali conversion is 2 to 4 hours, and the ball milling speed of the wet ball milling alkali conversion is 400 to 600 rpm.
[0033] Specifically, the main component of the primary defluorination slag and the secondary defluorination slag is magnesium fluoride. By adding sodium hydroxide to the magnesium fluoride for wet ball milling, the magnesium fluoride can be converted into magnesium hydroxide. The obtained magnesium hydroxide is reused in the primary defluorination and secondary defluorination processes to achieve the recycling of magnesium hydroxide.
[0034] In order to further illustrate the technical solution of the present application in detail to support the technical problem to be solved by the present application, the preparation method is described below with specific examples, such as Examples 1 to 5.
[0035] Example 1
[0036] A comprehensive utilization method of acidic wastewater in the glass thinning industry specifically comprises the following steps:
[0037] S1, adding sodium fluoride to the fluosilicic acid circulating water, and then stirring at a stirring speed of 200 rpm for 0.2 hours at a temperature of 20° C. to obtain a first solid-liquid mixture, and performing solid-liquid separation on the first solid-liquid mixture to obtain sodium fluosilicate and a mixed acid solution; the amount of the sodium fluoride is 1.2 times the theoretical reaction molar ratio of the fluosilicic acid circulating water;
[0038] S2, adding magnesium hydroxide to the mixed acid solution obtained in S1, and then stirring at a stirring speed of 200 rpm for 0.2 hours at a temperature of 25° C. to obtain a second solid-liquid mixture, and performing solid-liquid separation on the second solid-liquid mixture to obtain a primary defluorination liquid and a primary defluorination slag; the amount of the magnesium hydroxide used is 0.8 times the theoretical reaction molar ratio of the mixed acid solution;
[0039] S3, mixing the primary defluorination liquid obtained in S2 with the acidic spray liquid, then adding magnesium hydroxide, stirring at a temperature of 50° C. and a stirring speed of 200 rpm for 1 hour to obtain a third solid-liquid mixture, and performing solid-liquid separation on the third solid-liquid mixture to obtain a secondary defluorination liquid and a secondary defluorination slag; the volume ratio of the primary defluorination liquid to the acidic spray liquid is 1:3; the amount of magnesium hydroxide added is 1.4 times the theoretical reaction molar ratio of the primary defluorination liquid to the acidic spray liquid;
[0040] S4, adding calcium oxide to the secondary defluorination liquid obtained in S3, adjusting the pH to 5.5, stirring at a temperature of 15° C. until no solid precipitate is generated, obtaining a fourth solid-liquid mixture, and subjecting the fourth solid-liquid mixture to solid-liquid separation to obtain deep defluorination slag and qualified tail liquid; the amount of calcium oxide added is 1.2 times the reaction molar ratio of fluoride ions;
[0041] S5, mixing the primary defluorination slag obtained in S2 with the secondary defluorination slag obtained in S3, then adding sodium hydroxide, performing wet ball milling alkali conversion to obtain magnesium hydroxide and alkali conversion liquid, and then recycling the magnesium hydroxide to S2 and S3; the amount of sodium hydroxide used is 1 times the theoretical reaction molar ratio of magnesium fluoride in the primary defluorination slag and the secondary defluorination slag; the ball-to-material ratio of the wet ball milling alkali conversion is 8, the solid-liquid ratio of the wet ball milling alkali conversion is 1 mL / g, the ball milling time of the wet ball milling alkali conversion is 2 hours, and the ball milling speed of the wet ball milling alkali conversion is 400 rpm;
[0042] S6, adding hydrofluoric acid to the alkali liquid obtained in S5 for neutralization to obtain a neutralized liquid;
[0043] S7, evaporating and crystallizing the neutralized solution obtained in S6 to obtain sodium fluoride and a crystallization mother liquor, wherein the sodium fluoride is recycled to S1, and the crystallization mother liquor is returned to S5 for wet ball milling alkali conversion.
[0044] Example 2
[0045] A comprehensive utilization method of acidic wastewater in the glass thinning industry specifically comprises the following steps:
[0046] S1, adding sodium fluoride to the fluosilicic acid circulating water, and then stirring at a temperature of 40° C. and a stirring speed of 400 rpm for 2 hours to obtain a first solid-liquid mixture, and performing solid-liquid separation on the first solid-liquid mixture to obtain sodium fluosilicate and a mixed acid solution; the amount of the sodium fluoride is 1.6 times the theoretical reaction molar ratio of the fluosilicic acid circulating water;
[0047] S2, adding magnesium hydroxide to the mixed acid solution obtained in S1, and then stirring at a temperature of 50° C. and a stirring speed of 400 rpm for 2 hours to obtain a second solid-liquid mixture, and performing solid-liquid separation on the second solid-liquid mixture to obtain a primary defluorination liquid and a primary defluorination slag; the amount of the magnesium hydroxide used is 1.2 times the theoretical reaction molar ratio of the mixed acid solution;
[0048] S3, mixing the primary defluorination liquid obtained in S2 with the acidic spray liquid, then adding magnesium hydroxide, stirring at a temperature of 50° C. and a stirring speed of 400 rpm for 2 hours to obtain a third solid-liquid mixture, and performing solid-liquid separation on the third solid-liquid mixture to obtain a secondary defluorination liquid and a secondary defluorination slag; the volume ratio of the primary defluorination liquid to the acidic spray liquid is 1:6; the amount of magnesium hydroxide added is 1.6 times the theoretical reaction molar ratio of the primary defluorination liquid to the acidic spray liquid;
[0049] S4, adding calcium oxide to the secondary defluorination liquid obtained in S3, adjusting the pH to 8.0, stirring at a temperature of 35° C. until no solid precipitate is generated, obtaining a fourth solid-liquid mixture, and subjecting the fourth solid-liquid mixture to solid-liquid separation to obtain deep defluorination slag and qualified tail liquid; the amount of calcium oxide added is 1.6 times the molar ratio of the fluoride ion reaction;
[0050] S5, mixing the primary defluorination slag obtained in S2 with the secondary defluorination slag obtained in S3, then adding sodium hydroxide, performing wet ball milling alkali conversion to obtain magnesium hydroxide and alkali conversion liquid, and then recycling the magnesium hydroxide to S2 and S3; the amount of sodium hydroxide used is twice the theoretical reaction molar ratio of magnesium fluoride in the primary defluorination slag and the secondary defluorination slag; the ball-to-material ratio of the wet ball milling alkali conversion is 12, the solid-liquid ratio of the wet ball milling alkali conversion is 4 mL / g, the ball milling time of the wet ball milling alkali conversion is 2 hours, and the ball milling speed of the wet ball milling alkali conversion is 600 rpm;
[0051] S6, adding hydrofluoric acid to the alkali liquid obtained in S5 for neutralization to obtain a neutralized liquid;
[0052] S7, evaporating and crystallizing the neutralized solution obtained in S6 to obtain sodium fluoride and a crystallization mother liquor, wherein the sodium fluoride is recycled to S1, and the crystallization mother liquor is returned to S5 for wet ball milling alkali conversion.
[0053] Example 3
[0054] A comprehensive utilization method of acidic wastewater in the glass thinning industry specifically comprises the following steps:
[0055] S1, adding sodium fluoride to the fluosilicic acid circulating water, and then stirring at a temperature of 30° C. and a stirring speed of 400 rpm for 1 hour to obtain a first solid-liquid mixture, and performing solid-liquid separation on the first solid-liquid mixture to obtain sodium fluosilicate and a mixed acid solution; the amount of the sodium fluoride is 1.4 times the theoretical reaction molar ratio of the fluosilicic acid circulating water;
[0056] S2, adding magnesium hydroxide to the mixed acid solution obtained in S1, and then stirring at a temperature of 50° C. and a stirring speed of 400 rpm for 1 hour to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag; the amount of the magnesium hydroxide used is 1 times the theoretical reaction molar ratio of the mixed acid solution;
[0057] S3, mixing the primary defluorination liquid obtained in S2 with the acidic spray liquid, then adding magnesium hydroxide, stirring at a temperature of 50° C. and a stirring speed of 400 rpm for 2 hours to obtain a third solid-liquid mixture, and performing solid-liquid separation on the third solid-liquid mixture to obtain a secondary defluorination liquid and a secondary defluorination slag; the volume ratio of the primary defluorination liquid to the acidic spray liquid is 1:5; the amount of magnesium hydroxide added is 1.5 times the theoretical reaction molar ratio of the primary defluorination liquid to the acidic spray liquid;
[0058] S4, adding calcium oxide to the secondary defluorination liquid obtained in S3, adjusting the pH to 7, stirring at a temperature of 20° C. until no solid precipitate is generated, obtaining a fourth solid-liquid mixture, and subjecting the fourth solid-liquid mixture to solid-liquid separation to obtain deep defluorination slag and qualified tail liquid; the amount of calcium oxide added is 1.5 times the molar ratio of the fluoride ion reaction;
[0059] S5, the primary defluorination slag obtained in S2 is mixed with the secondary defluorination slag obtained in S3, and then sodium hydroxide is added to perform wet ball milling alkali conversion to obtain magnesium hydroxide and alkali conversion liquid, and then the magnesium hydroxide is recycled to S2 and S3; the amount of sodium hydroxide used is 1.8 times the theoretical reaction molar ratio of magnesium fluoride in the primary defluorination slag and the secondary defluorination slag; the ball-to-material ratio of the wet ball milling alkali conversion is 12, the solid-liquid ratio of the wet ball milling alkali conversion is 2mL / g, the ball milling time of the wet ball milling alkali conversion is 4 hours, and the ball milling speed of the wet ball milling alkali conversion is 600 rpm;
[0060] S6, adding hydrofluoric acid to the alkali liquid obtained in S5 for neutralization to obtain a neutralized liquid;
[0061] S7, evaporating and crystallizing the neutralized solution obtained in S6 to obtain sodium fluoride and a crystallization mother liquor, wherein the sodium fluoride is recycled to S1, and the crystallization mother liquor is returned to S5 for wet ball milling alkali conversion.
[0062] Example 4
[0063] A comprehensive utilization method of acidic wastewater in the glass thinning industry specifically comprises the following steps:
[0064] S1, adding sodium fluoride to the fluosilicic acid circulating water, and then stirring at a temperature of 40° C. and a stirring speed of 400 rpm for 1 hour to obtain a first solid-liquid mixture, and performing solid-liquid separation on the first solid-liquid mixture to obtain sodium fluosilicate and a mixed acid solution; the amount of the sodium fluoride is 1.6 times the theoretical reaction molar ratio of the fluosilicic acid circulating water;
[0065] S2, adding magnesium hydroxide to the mixed acid solution obtained in S1, and then stirring at a stirring speed of 400 rpm for 1.5 hours at a temperature of 35° C. to obtain a second solid-liquid mixture, and performing solid-liquid separation on the second solid-liquid mixture to obtain a primary defluorination liquid and a primary defluorination slag; the amount of the magnesium hydroxide used is 1.2 times the theoretical reaction molar ratio of the mixed acid solution;
[0066] S3, mixing the primary defluorination liquid obtained in S2 with the acidic spray liquid, then adding magnesium hydroxide, stirring at a temperature of 50°C and a stirring speed of 200-400 rpm for 2 hours to obtain a third solid-liquid mixture, and performing solid-liquid separation on the third solid-liquid mixture to obtain a secondary defluorination liquid and a secondary defluorination slag; the volume ratio of the primary defluorination liquid to the acidic spray liquid is 1:4; the amount of magnesium hydroxide added is 1.4 times the theoretical reaction molar ratio of the primary defluorination liquid to the acidic spray liquid;
[0067] S4, adding calcium oxide to the secondary defluorination liquid obtained in S3, adjusting the pH to 6, stirring at a temperature of 35° C. until no solid precipitate is generated, obtaining a fourth solid-liquid mixture, and subjecting the fourth solid-liquid mixture to solid-liquid separation to obtain deep defluorination slag and qualified tail liquid; the amount of deep calcium oxide added is 1.4 times the molar ratio of the fluoride ion reaction;
[0068] S5, the primary defluorination slag obtained in S2 is mixed with the secondary defluorination slag obtained in S3, and then sodium hydroxide is added to perform wet ball milling alkali conversion to obtain magnesium hydroxide and alkali conversion liquid, and then the magnesium hydroxide is recycled to S2 and S3; the amount of sodium hydroxide used is 1.8 times the theoretical reaction molar ratio of magnesium fluoride in the primary defluorination slag and the secondary defluorination slag; the ball-to-material ratio of the wet ball milling alkali conversion is 10, the solid-liquid ratio of the wet ball milling alkali conversion is 4 mL / g, the ball milling time of the wet ball milling alkali conversion is 3 hours, and the ball milling speed of the wet ball milling alkali conversion is 500 rpm;
[0069] S6, adding hydrofluoric acid to the alkali liquid obtained in S5 for neutralization to obtain a neutralized liquid;
[0070] S7, evaporating and crystallizing the neutralized solution obtained in S6 to obtain sodium fluoride and a crystallization mother liquor, wherein the sodium fluoride is recycled to S1, and the crystallization mother liquor is returned to S5 for wet ball milling alkali conversion.
[0071] Example 5
[0072] A comprehensive utilization method of acidic wastewater in the glass thinning industry specifically comprises the following steps:
[0073] S1, adding sodium fluoride to the fluosilicic acid circulating water, and then stirring at a temperature of 30° C. and a stirring speed of 300 rpm for 1.5 hours to obtain a first solid-liquid mixture, and performing solid-liquid separation on the first solid-liquid mixture to obtain sodium fluosilicate and a mixed acid solution; the amount of the sodium fluoride is 1.4 times the theoretical reaction molar ratio of the fluosilicic acid circulating water;
[0074] S2, adding magnesium hydroxide to the mixed acid solution obtained in S1, and then stirring at a stirring speed of 300 rpm at a temperature of 40° C. for 1.2 hours to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag; the amount of the magnesium hydroxide used is 1 times the theoretical reaction molar ratio of the mixed acid solution;
[0075] S3, mixing the primary defluorination liquid obtained in S2 with the acidic spray liquid, then adding magnesium hydroxide, stirring at a temperature of 40°C and a stirring speed of 300 rpm for 2 hours to obtain a third solid-liquid mixture, and performing solid-liquid separation on the third solid-liquid mixture to obtain a secondary defluorination liquid and a secondary defluorination slag; the volume ratio of the primary defluorination liquid to the acidic spray liquid is 1:5; the amount of magnesium hydroxide added is 1.4 times the theoretical reaction molar ratio of the primary defluorination liquid to the acidic spray liquid;
[0076] S4, adding calcium oxide to the secondary defluorination liquid obtained in S3, adjusting the pH to 7.5, stirring at a temperature of 25° C. until no solid precipitate is generated, obtaining a fourth solid-liquid mixture, and subjecting the fourth solid-liquid mixture to solid-liquid separation to obtain deep defluorination slag and qualified tail liquid; the amount of calcium oxide added is 1.5 times the molar ratio of the fluoride ion reaction;
[0077] S5, mixing the primary defluorination slag obtained in S2 with the secondary defluorination slag obtained in S3, then adding sodium hydroxide, performing wet ball milling alkali conversion to obtain magnesium hydroxide and alkali conversion liquid, and then recycling the magnesium hydroxide to S2 and S3; the amount of sodium hydroxide used is 1.5 times the theoretical reaction molar ratio of magnesium fluoride in the primary defluorination slag and the secondary defluorination slag; the ball-to-material ratio of the wet ball milling alkali conversion is 10, the solid-liquid ratio of the wet ball milling alkali conversion is 2mL / g, the ball milling time of the wet ball milling alkali conversion is 4 hours, and the ball milling speed of the wet ball milling alkali conversion is 400 rpm;
[0078] S6, adding hydrofluoric acid to the alkali liquid obtained in S5 for neutralization to obtain a neutralized liquid;
[0079] S7, evaporating and crystallizing the neutralized solution obtained in S6 to obtain sodium fluoride and a crystallization mother liquor, wherein the sodium fluoride is recycled to S1, and the crystallization mother liquor is returned to S5 for wet ball milling alkali conversion.
[0080] The effects of treating wastewater from the glass thinning industry by Examples 1 to 5 are compared as follows:
[0081] Test of H2SiF6 removal rate in fluorosilicic acid circulating water: The concentration of H2SiF6 in fluorosilicic acid circulating water was tested before and after treatment. The removal rate of H2SiF6 was calculated based on the concentration of H2SiF6 before and after treatment. The results are shown in Table 1.
[0082] Table 1 Removal rate of H2SiF6 in fluorosilicic acid circulating water
[0083] Example <![CDATA[Removal rate of H2SiF6 / %]]> Example 1 98.6 Example 2 99.3 Example 3 98.9 Example 4 99.1 Example 5 98.8
[0084] Test on the mass concentration of fluoride ions in qualified tail liquid: Take qualified tail liquid to test the fluoride ion concentration. The test results are shown in Table 2.
[0085] Table 2 Mass concentration of fluoride ions in qualified tail liquid
[0086] Example Fluoride ion concentration / (mg / L) Example 1 4 Example 2 3 Example 3 5 Example 4 6 Example 5 5
[0087] According to the data in Tables 1 and 2, by using a comprehensive utilization method of acidic wastewater in the glass thinning industry to treat the fluorosilicic acid circulating water generated in the glass thinning industry, the removal rate of H2SiF6 can reach 99.3%, and the maximum mass concentration of fluoride ions in the discharged tail liquid is 6 mg / L, which can effectively remove fluoride ions in the fluorosilicic acid circulating water.
[0088] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A comprehensive utilization method of acidic wastewater in glass thinning industry, characterized in that: The comprehensive utilization method of acidic wastewater in the glass thinning industry specifically includes: S1, precipitation: adding sodium fluoride to the fluorosilicic acid circulating water, stirring to obtain a first solid-liquid mixture, and performing solid-liquid separation on the first solid-liquid mixture to obtain sodium fluorosilicate and a mixed acid solution; S2, primary defluorination: adding magnesium hydroxide to the mixed acid solution obtained in S1, stirring to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag; S3, secondary defluorination: the primary defluorination liquid obtained in S2 is mixed with the spray liquid, and then magnesium hydroxide is added, stirred to obtain a third solid-liquid mixture, and the third solid-liquid mixture is subjected to solid-liquid separation to obtain a secondary defluorination liquid and a secondary defluorination slag; S4, deep defluorination: adding a deep defluorination agent to the secondary defluorination liquid obtained in S3, adjusting the pH value, and obtaining deep defluorination slag and qualified tail liquid; S5, wet ball milling alkali conversion: the primary defluorination residue obtained in S2 is mixed with the secondary defluorination residue obtained in S3, and then sodium hydroxide is added to perform wet ball milling alkali conversion to obtain magnesium hydroxide and alkali conversion liquid, and then the magnesium hydroxide is recycled to S2 and S3; S6, neutralization: adding hydrofluoric acid to the alkaline liquid obtained in S5 for neutralization to obtain a neutralized liquid; S7, evaporation crystallization: the neutralized solution obtained in S6 is evaporated and crystallized to obtain sodium fluoride and a crystallization mother liquor, the sodium fluoride is recycled to S1, and the crystallization mother liquor is returned to S5 for wet ball milling alkali conversion.
2. A comprehensive utilization method of acidic wastewater in glass thinning industry as claimed in claim 1, characterized in that: The method of adding sodium fluoride to the fluorosilicic acid circulating water to obtain a first solid-liquid mixture, and subjecting the first solid-liquid mixture to solid-liquid separation to obtain sodium fluorosilicate and a mixed acid solution specifically comprises: adding sodium fluoride to the fluorosilicic acid circulating water, and then stirring at a stirring speed of 200 to 400 rpm for 0.2 to 2 hours at a temperature of 20 to 40° C. to obtain a first solid-liquid mixture, and subjecting the first solid-liquid mixture to solid-liquid separation to obtain sodium fluorosilicate and a mixed acid solution; the amount of sodium fluoride used is 1.2 to 1.6 times the theoretical reaction molar ratio of the fluorosilicic acid circulating water.
3. A comprehensive utilization method of acidic wastewater in glass thinning industry as claimed in claim 1, characterized in that: The method of adding magnesium hydroxide to the mixed acid solution obtained in S1, stirring to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag specifically comprises: adding magnesium hydroxide to the mixed acid solution obtained in S1, and then stirring at a stirring speed of 200 to 400 rpm for 0.2 to 2 hours at a temperature of 25 to 50° C. to obtain a second solid-liquid mixture, and subjecting the second solid-liquid mixture to solid-liquid separation to obtain a primary defluorination liquid and a primary defluorination slag.
4. A comprehensive utilization method of acidic wastewater in glass thinning industry as claimed in claim 3, characterized in that: The dosage of the magnesium hydroxide is 0.8 to 1.2 times the theoretical reaction molar ratio of the mixed acid solution.
5. The comprehensive utilization method of acidic wastewater in glass thinning industry according to claim 1, characterized in that: The step of mixing the primary defluorination liquid obtained in S2 with the spray liquid, then adding magnesium hydroxide, stirring to obtain a third solid-liquid mixture, and subjecting the third solid-liquid mixture to solid-liquid separation to obtain a secondary defluorination liquid and a secondary defluorination slag specifically comprises: mixing the primary defluorination liquid obtained in S2 with the spray liquid, then adding magnesium hydroxide, stirring at a temperature of 25 to 50° C. and a stirring speed of 200 to 400 rpm for 0.2 to 2 hours to obtain a third solid-liquid mixture, and subjecting the third solid-liquid mixture to solid-liquid separation to obtain a secondary defluorination liquid and a secondary defluorination slag.
6. A comprehensive utilization method of acidic wastewater in glass thinning industry as claimed in claim 5, characterized in that: The volume ratio of the primary defluorination liquid to the spray liquid is 1:3 to 1:6; the amount of magnesium hydroxide added is 1.2 to 1.6 times the theoretical reaction molar ratio of the primary defluorination liquid to the spray liquid; and the spray liquid is an acidic spray liquid.
7. A comprehensive utilization method of acidic wastewater in glass thinning industry as claimed in claim 1, characterized in that: The step of adding a deep defluorination agent to the secondary defluorination liquid obtained in S3 to obtain a deep defluorination slag and a qualified tail liquid specifically comprises: adding a deep defluorination agent to the secondary defluorination liquid obtained in S3, adjusting the pH to 5.5-8.0, stirring at a temperature of 15-35° C. until no solid precipitate is generated to obtain a fourth solid-liquid mixture, and performing solid-liquid separation on the fourth solid-liquid mixture to obtain a deep defluorination slag and a qualified tail liquid.
8. A comprehensive utilization method of acid wastewater from glass thinning industry as claimed in claim 7, characterized in that: The added amount of the deep defluorination agent is 1.2 to 1.6 times the reaction molar ratio of fluoride ions; the deep defluorination agent is calcium oxide.
9. The comprehensive utilization method of acid wastewater in glass thinning industry according to claim 1, characterized in that: In S5, the amount of sodium hydroxide used is 1 to 2 times the theoretical reaction molar ratio of magnesium fluoride in the primary defluorination slag and the secondary defluorination slag.
10. The comprehensive utilization method of acid wastewater in glass thinning industry according to claim 1, characterized in that: In S5, the ball-to-material ratio of the wet ball milling alkali rotation is 8-12, the solid-liquid ratio of the wet ball milling alkali rotation is 1-4 mL / g, the ball milling time of the wet ball milling alkali rotation is 2-4 hours, and the ball milling speed of the wet ball milling alkali rotation is 400-600 rpm.
Citation Information
Cited By
Treatment method for high-concentration fluorine-containing wastewater of glass factory
CN120987442A