Special high-impact transparent polypropylene material and production method thereof

Through the polymerization process of the liquid phase loop pipe and the gas phase reactor, the hydrogen and ethylene content is controlled, and the high production cost and processing difficulty of high impact transparent polypropylene are solved, and low haze, high transparency and impact resistance are achieved. Polypropylene products, suitable for low-temperature food packaging.

CN119039497APending Publication Date: 2024-11-29NORTH HUAJIN CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411116490.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing high impact transparent polypropylene production methods have problems such as high cost, high processing difficulty, reduced transparency and rigidity, and it is difficult to achieve large-scale production.

Method used

The polymerization process of the series liquid phase loop reactor and gas phase reactor is adopted to control the hydrogen flow rate and ethylene content to ensure the molecular weight distribution and melt flow rate of polypropylene, combined with the two-step process of flash and steam, reduce the monomer Consumption and improve product impact resistance and optical properties.

Benefits of technology

The low haze, high transparency and good impact resistance of high impact transparent polypropylene is achieved, which reduces production costs and solves the problem that materials are prone to brittle and easily cracked at low temperatures in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993770890000061
    Figure BDA0004993770890000061
  • Figure BDA0004993770890000071
    Figure BDA0004993770890000071
  • Figure BDA0004993770890000081
    Figure BDA0004993770890000081
Patent Text Reader

Abstract

The invention relates to the technical field of macromolecules, and particularly discloses a high-impact transparent polypropylene special material and a production method thereof. According to the invention, an improved Spheripol polypropylene production process is adopted, a spherical catalyst is adopted to control the form of a polymer, the catalytic efficiency is high, and the polymerization particle size is uniform; the product of the high-impact transparent polypropylene special material produced by the process has the advantages of high impact property, low haze, good uniformity and consistency, capability of meeting the performance requirements of home furnishing and low-temperature food packaging by various performance indexes, good uniformity, good optical performance, no peculiar smell and the like, and can realize large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymers, and specifically discloses a special material for high-impact transparent polypropylene and a production method. Background Art

[0002] There are two main methods for producing high-impact transparent polypropylene: one is direct polymerization; the other is to blend random copolymer polypropylene with transparent elastomers to improve its impact strength while ensuring the transparency of random copolymer polypropylene. At present, the main method is to blend random polypropylene with elastomers such as POE, POP, SEBS, etc. This method can improve the impact resistance of the material to a certain extent, but it also brings many adverse effects, such as: the added elastomer is expensive and needs to be granulated by a twin-screw extruder, which will greatly increase the production cost. At the same time, the product modified by adding elastomer will increase the haze and reduce the rigidity, which greatly affects the transparency and rigidity of the product, and increases the processing difficulty and prolongs the processing cycle. The introduction of elastomers also reduces the sanitation of the material, and its application in medical and food packaging fields is limited. Therefore, the direct polymerization method is more economical and scalable.

[0003] High-impact transparent polypropylene has excellent transparency, excellent room temperature and low temperature impact resistance, heat resistance and good processing performance, which can meet the market demand for transparent packaging of frozen foods. This product is mainly used in large storage boxes, syringes, hollow blow molding bottle packaging, ice cream boxes, frozen food packaging boxes, low-temperature storage boxes, etc.

[0004] At present, although there are studies on high-impact transparent polypropylene special materials in domestic and foreign patents, the preparation process is difficult and cannot be mass-produced. Therefore, it is necessary to study the production process of high-impact transparent polypropylene resin to produce products with high impact resistance, low haze, good uniformity and consistency, and various performance indicators meet the performance requirements of household and low-temperature food packaging. Summary of the invention

[0005] The technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides a production process technology for a high-impact transparent polypropylene special material, which specifically comprises the following steps:

[0007] S1. Injecting polymerization-grade propylene into a polymerization reactor R200, adding a configured main catalyst, a co-catalyst, and an external electron donor to perform a prepolymerization reaction to obtain a prepolymer; the main catalyst comprises TiCl4, MgCl2, and an internal electron donor; the co-catalyst comprises triethylaluminum; the temperature of the prepolymerization reactor R200 is 18 to 20°C; the reaction time is 10 to 18 min;

[0008] S2. After the prepolymerization reaction, the prepolymer enters the loop reactor for polymerization reaction, the prepolymer reacts with propylene monomer, hydrogen and ethylene, and the loop reactor is polymerized to obtain a random copolymer; the reaction temperature of the loop reactor R201 / R202 is controlled to be 67-70°C, and the slurry density is 480-530kg / m 3 , the pressure is 3.0~4.0MPa; the ethylene content in the loop is 1.0~3.0%. Hydrogen, as a chain transfer agent for polymerization reaction, has the function of adjusting molecular weight and controlling melt index. Hydrogen is added differentially in two loop reactors. During production, the hydrogen flow rate of loop reactor R201 is controlled to be 1000~5000g / h according to the target index, and the hydrogen flow rate of loop reactor R202 is controlled to be 1000~5000g / h, and the reaction time is 1.5~2h;

[0009] S3. The random copolymer produced by the loop reactor R201 / R202 is vaporized in the flash tank D301 and then enters the gas phase reactor R401; in the gas phase reactor, it undergoes block copolymerization with ethylene and propylene, and the produced dimer mainly composed of ethylene-propylene rubber mainly grows in the sphere of the homopolymer, and finally a mixture of homopolymer and dimer with an island-in-sea structure is obtained; the temperature of the gas phase reactor R401 is controlled to be 75-80°C, the pressure to be 1.25-1.37MPa, the ethylene content to be 1.0-3.0% (w), the ethylene / (ethylene+propylene) molar ratio to be 0.20-0.40, and the reaction time to be 25-45min.

[0010] S4. The impact copolymer generated in the gas phase reactor R401 is further separated from the propylene monomer by a low-pressure bag filter F301, and the separated polypropylene powder enters the steamer D501 and contacts with low-pressure steam to remove hydrocarbons and decompose the catalyst, triethyl aluminum, and electron donor remaining in the polymer;

[0011] S5. The polymer powder from the steamer D501 is dried by high-temperature nitrogen in the dryer D502 to remove excess moisture. The polypropylene powder from the dryer D502 is added with antioxidants, nucleating agents, and halogen absorbers in the heating cylinder. The heating cylinder temperature of the extruder is controlled at 220-230°C, and mixed and processed into polypropylene pellets.

[0012] Preferably, in step S1: the Ti active material contained in the main catalyst accounts for 2.0% to 3.0% of the weight of the main catalyst; the co-catalyst includes triethylaluminum; the main catalyst is added in an amount of 2.0 to 6.0 L / h; the external electron donor is added in an amount of 1.0 to 2.0 kg / h; the co-catalyst triethylaluminum is added in an amount of 5.0 to 9.0 kg / h, so as to reduce the residual aluminum in the product.

[0013] Preferably, the internal electron donor in the catalyst is selected from 2,2-dialkyl-1,3-dialkoxypropane, 2,2-dialkyl-1,3-diisobutylpropane, 2,2-dicyclopentyl-1,3-dimethoxypropane, 2-ethyl-2-butyl-1,3-dimethoxypropane, 2-ethylhexyl phthalate, diisobutyl phthalate, ethyl phthalate, and dibutyl phthalate.

[0014] Preferably, the external electron donor selection range includes cyclohexylmethyldimethoxysilane, diphenyldimethoxysilane, diisobutyldimethoxysilane, dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, and tetraethoxysilane.

[0015] Preferably, the antioxidant is one or more of antioxidant 1010, antioxidant 1076, antioxidant 168, antioxidant 3114, antioxidant 626, and antioxidant 264.

[0016] Preferably, the halogen absorber is calcium stearate or zinc stearate.

[0017] Preferably, the nucleating agent is a sorbitol nucleating agent; the dosage of the nucleating agent is 1000-2000 ppm.

[0018] Preferably, the propylene is removed from impurities and regenerated by a propylene refining unit before use. Trace amounts of harmful impurities in propylene will destroy the activity and directional ability of the catalyst and weaken the polymerization reaction system. Therefore, it is necessary to strengthen the refining and quality monitoring of propylene to reduce the impact of trace amounts of harmful impurities on the catalyst and improve product quality.

[0019] Preferably, the antioxidant is used in an amount of 1000 to 3000 ppm; the halogen absorbent is used in an amount of 1000 to 3000 ppm.

[0020] In a second aspect, the present invention provides a high-impact transparent polypropylene special material, which is prepared by the method described in the first aspect.

[0021] The idea of ​​the present invention is:

[0022] The polypropylene device is a series polymerization of two liquid phase loop reactors and one gas phase reactor. The first two loop reactors in the series process are liquid phase random copolymerization, and the last gas phase reactor is gas phase copolymerization. The molecular weight distribution of polypropylene is ensured by controlling the amount of hydrogen added to the two loop reactors and the gas phase reactor respectively. The loop reactor is combined with the gas phase reactor. Flash evaporation is used to evaporate propylene. The polymer is treated by a two-step method of steaming and drying, and the steam in the steaming tail gas is condensed to separate pure hydrocarbon monomers, which can completely recycle the hydrocarbons in the tail gas and reduce the consumption of monomers.

[0023] The melt flow rate of polypropylene is controlled by the hydrogen introduced during the polymerization reaction. In order to ensure that the polypropylene product has a certain melt flow rate, a production method of adjusting the melt flow rate with hydrogen without using a degradation agent is adopted. Hydrogen is used as a chain transfer agent for the polymerization reaction. It is dissolved in liquid propylene and enters the loop reactor R201 / R202 for chain transfer reaction. The greater the amount of hydrogen added, the higher the melt flow rate of the product, the smaller the molecular weight of the polymer, and the product has the characteristics of being non-toxic and odorless.

[0024] High-impact transparent polypropylene products must have good mechanical and optical properties, including impact strength and haze, to ensure the stability of polypropylene products. Accurately controlling the temperature of each reactor is very critical in the production process to ensure that the mechanical and optical properties of the polypropylene products produced are optimal.

[0025] The toughness of polypropylene is determined by the ethylene content, so the higher the ethylene content of the product, the better the toughness. The impact strength of polypropylene products can be improved from the following two aspects. According to the polymerization reaction, the ethylene content is slowly increased to the target value to improve the impact strength of the product; the ethylene content of the loop reactor is slowly increased to increase the ethylene content in the loop reactor within the control range of 1.0-3.0%. The gas phase reactor is controlled at 1.0-3.0%, and the content of ethylene-propylene rubber in the gas phase reactor is increased. The high-impact transparent polypropylene products produced have high impact resistance, and the room temperature cantilever beam impact strength is ≥7kJ / m 2 .

[0026] In order to ensure that the high-impact transparent polypropylene has good optical properties and good processing properties, the polypropylene produced is copolymerized polypropylene, and the process parameters of each reactor are adjusted to improve the optical properties of the polypropylene product from the following two aspects. The ethylene content of the loop reactor and the molar ratio of ethylene / (ethylene+propylene) of the gas phase reactor are strictly controlled to ensure the transparency of the impact-resistant copolymerized polypropylene, and the particle size of the rubber particles is less than 0.4μm; sorbitol nucleating agents are added in the granulation stage to further improve the optical properties of polypropylene. The haze of the produced high-impact transparent polypropylene is ≤15%, and the product has good optical properties.

[0027] Beneficial effects achieved by the present invention:

[0028] The present invention produces high-impact transparent polypropylene by direct polymerization, which has both transparency and impact resistance, reduces product haze, improves transparency, and has good impact resistance, solves the problem that traditional transparent polypropylene is easy to become brittle and crack at low temperatures, and reduces the production cost of downstream customers. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the following examples. It should be noted that the present invention is not limited to the following examples.

[0030] Example 1

[0031] ZN catalyst was used, in which the electron donor in the main catalyst was diisobutyl phthalate, the Ti content was 2.6% (w), the Mg content was 14.2% (w), and the main catalyst addition amount was 3.5L / h; the co-catalyst was triethylaluminum, and the addition amount was 5.3kg / h; the external electron donor was cyclohexylmethyldimethoxysilane, and the addition amount was 2.1kg / h. The temperature of the prepolymerization reactor R200 was 20°C, the propylene feed amount was 2100kg / h, and the reaction time was 13min. The propylene feed amount of the loop reactor R201 / R202 was 29500 / 10200kg / h, the temperature was 68.5 / 68.5°C, and the slurry density was 490 / 490kg / m 3 , pressure is 3.90 / 3.90MPa, ethylene content is 1.1 / 1.1% (w), reaction time is 1.4h. The feed rate of gas phase reactor R401 is 4100kg / h, the temperature is 78.0℃, the pressure is 1.35MPa, and the ethylene content is 2.8% (w). The polypropylene powder is added to the extruder with the added composite antioxidants 1010 and 168 (mass ratio 1:1), the dosage is 1840ppm, the dosage of sorbitol nucleating agent NX8000K is 1400ppm, and the dosage of calcium stearate is 1550ppm. Control the heating barrel temperature of the extruder to 220℃:

[0032] Table 1: Test results of polypropylene performance in Example 1

[0033] Test Name unit Performance Indicators Melt flow rate g / 10min 16.4 Izod impact strength (23℃) <![CDATA[kJ / m 2 ]]> 8.7 Izod impact strength (0℃) <![CDATA[kJ / m 2 ]]> 5.4 Flexural modulus MPa 1102 Haze % 12.3

[0034] Example 2

[0035] ZN catalyst was used, in which the electron donor in the main catalyst was 2,2-dialkyl-1,3-dialkoxypropane, the Ti content was 2.3% (w), the Mg content was 13.3% (w), and the main catalyst addition amount was 4.4L / h; the co-catalyst was triethylaluminum, and the addition amount was 4.3kg / h; the external electron donor was cyclohexyldimethoxysilane, and the addition amount was 2.5kg / h. The temperature of the prepolymerization reactor R200 was 19.5°C, the propylene feed amount was 1930kg / h, and the reaction time was 12min. The propylene feed amount of the loop reactor R201 / R202 was 31300 / 11600kg / h, the temperature was 69.5 / 69.5°C, and the slurry density was 490 / 490kg / m 3, pressure is 3.93 / 3.93MPa, ethylene content is 1.3 / 1.3% (w), reaction time is 1.7h. The feed rate of gas phase reactor R401 is 4100kg / h, the temperature is 80.0℃, the pressure is 1.37MPa, and the ethylene content is 2.5% (w). The polypropylene powder is added with composite antioxidants 3114 and 626 (mass ratio 1:2) in the extruder, the dosage is 1250ppm, the dosage of sorbitol nucleating agent NX8000K is 1650ppm, and the dosage of calcium stearate is 1400ppm. The heating cylinder temperature is controlled to 230℃, and the mixed processing is high impact transparent polypropylene. The performance test is shown in Table 2:

[0036] Table 2 Example 2 Polypropylene performance test results

[0037]

[0038] Example 3

[0039] ZN catalyst was used, in which the electron donor in the main catalyst was 2,2-dialkyl-1,3-dialkoxypropane, the Ti content was 2.7% (w), the Mg content was 13.8% (w), and the main catalyst addition amount was 3.9L / h; the co-catalyst was triethylaluminum, and the addition amount was 6.3kg / h; the external electron donor was dicyclopentyldimethoxysilane, and the addition amount was 2.1kg / h. The temperature of the prepolymerization reactor R200 was 19.1°C, the propylene feed amount was 2050kg / h, and the reaction time was 15min. The propylene feed amount of the loop reactor R201 / R202 was 32200 / 11900kg / h, the temperature was 69.2 / 69.2°C, and the slurry density was 507 / 507kg / m 3 , pressure is 4.0 / 3.95MPa, ethylene content is 1.5 / 1.5% (w), and reaction time is 1.5h. The feed rate of gas phase reactor R401 is 3400kg / h, the temperature is 77.7℃, the pressure is 1.21MPa, and the ethylene content is 2.4% (w). The polypropylene powder is added with composite antioxidants 1010 and 1076 (mass ratio 1:2) in the extruder, the dosage is 2000ppm, the sorbitol nucleating agent NX8000K is 1200ppm, and the calcium stearate is 1500ppm. The heating barrel temperature of the extruder is controlled to 225℃, and the mixed processing is high impact transparent polypropylene. The performance test is shown in Table 3:

[0040] Table 3 Example 3 Polypropylene performance test results

[0041]

[0042] Example 4

[0043] ZN catalyst was used, in which the electron donor in the main catalyst was ethyl phthalate, the Ti content was 2.5% (w), the Mg content was 14% (w), and the main catalyst addition amount was 3.2L / h; the co-catalyst was triethylaluminum, and the addition amount was 5.5kg / h; the external electron donor was diisobutyldimethoxysilane, and the addition amount was 1.6kg / h. The temperature of the prepolymerization reactor R200 was 18.7°C, the propylene feed amount was 1930kg / h, and the reaction time was 14min. The propylene feed amount of the loop reactor R201 / R202 was 30200 / 10700kg / h, the temperature was 70.0 / 70.0°C, and the slurry density was 515 / 515kg / m 3 , pressure is 3.90 / 3.90MPa, ethylene content is 1.4 / 1.4% (w), and reaction time is 1.4h. The feed rate of gas phase reactor R401 is 3100kg / h, the temperature is 77.5℃, the pressure is 1.26MPa, and the ethylene content is 2.3% (w). The polypropylene powder is added with composite antioxidants 1010 and 264 (mass ratio 1:1) in the extruder, the dosage is 1800ppm, the dosage of sorbitol nucleating agent NX8000K is 1800ppm, and the dosage of calcium stearate is 1200ppm. The heating barrel temperature of the extruder is controlled to 220℃, and the mixed processing is high impact transparent polypropylene. The performance test is shown in Table 4:

[0044] Table 4 Example 4 Polypropylene performance test results

[0045]

[0046] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A production process technology for high impact transparent polypropylene special material, characterized in that: The specific steps include: S1. Propylene is injected into the polymerization reactor R200, and the configured main catalyst, co-catalyst and external electron donor are added to perform a prepolymerization reaction to obtain a prepolymer; the main catalyst comprises TiCl4, MgCl2, and an internal electron donor; the co-catalyst comprises triethylaluminum; the temperature of the prepolymerization reactor R200 is 18 to 20°C; the reaction time is 10 to 18 min; S2. After the prepolymerization reaction, the prepolymer enters the loop reactor for polymerization reaction, the prepolymer reacts with propylene monomer, hydrogen and ethylene, and the loop reactor is polymerized to obtain a random copolymer; the reaction temperature of the loop reactor R201 / R202 is controlled to be 67-70°C, and the slurry density is 480-530kg / m 3 , pressure is 3.0~4.0MPa; ethylene content in the loop is 1.0~3.0%; hydrogen flow rate of loop reactor R201 is 1000~5000g / h, hydrogen flow rate of loop reactor R202 is 1000~5000g / h, reaction time is 1.5~2h; S3. The random copolymer generated by the loop reactor R201 / R202 is vaporized in the flash tank D301 and enters the gas phase reactor R401; the temperature of the gas phase reactor R401 is controlled to be 75 to 80°C, the pressure is 1.25 to 1.37 MPa, the ethylene content is 1.0 to 3.0% (w), the ethylene / (ethylene + propylene) molar ratio is 0.20 to 0.40, and the reaction time is 25 to 45 min; S4. The impact copolymer generated by the gas phase reactor R401 is passed through a low-pressure bag filter F301, and the polypropylene powder is further separated from the propylene monomer, and the separated polypropylene powder enters the steamer D501 and contacts with low-pressure steam; S5. The polymer powder from the steamer D501 is heated and dried by high-temperature nitrogen in the dryer D502. Antioxidants, nucleating agents and halogen absorbers are added to the polypropylene powder from the dryer D502 in the heating cylinder. The heating cylinder temperature of the extruder is controlled at 220-230°C, and the mixture is processed into polypropylene pellets.

2. The production process technology of high impact transparent polypropylene special material according to claim 1 is characterized in that: In step S1: the Ti active material contained in the main catalyst accounts for 2.0% to 3.0% of the weight of the main catalyst; the co-catalyst includes triethylaluminum; the main catalyst is added in an amount of 2.0 to 6.0 L / h; the external electron donor is added in an amount of 1.0 to 2.0 kg / h; and the co-catalyst triethylaluminum is added in an amount of 5.0 to 9.0 kg / h.

3. The production process technology of high impact transparent polypropylene special material according to claim 1 is characterized in that: The internal electron donor in the catalyst can be selected from 2,2-dialkyl-1,3-dialkoxypropane, 2,2-dialkyl-1,3-diisobutylpropane, 2,2-dicyclopentyl-1,3-dimethoxypropane, 2-ethyl-2-butyl-1,3-dimethoxypropane, 2-ethylhexyl phthalate, diisobutyl phthalate, ethyl phthalate and dibutyl phthalate.

4. The production process technology of high impact transparent polypropylene special material according to claim 1 is characterized in that: The selection range of the external electron donor includes cyclohexylmethyldimethoxysilane, diphenyldimethoxysilane, diisobutyldimethoxysilane, dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, and tetraethoxysilane.

5. The production process technology of high impact transparent polypropylene special material according to claim 1 is characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 1076, antioxidant 168, antioxidant 3114, antioxidant 626, and antioxidant 264.

6. The production process technology of high impact transparent polypropylene special material according to claim 1 is characterized in that: The halogen absorber is calcium stearate or zinc stearate.

7. The production process of high impact transparent polypropylene special material according to claim 1, characterized in that: The nucleating agent is a sorbitol nucleating agent; the dosage of the nucleating agent is 1000-2000ppm.

8. The production process technology of high impact transparent polypropylene special material according to claim 1 is characterized in that: The propylene is passed through a propylene refinement unit to remove impurities from the propylene and to be regenerated before use.

9. The production process technology of high impact transparent polypropylene special material according to claim 1 is characterized in that: The dosage of the antioxidant is 1000-3000ppm; the dosage of the halogen absorbent is 1000-3000ppm.

10. A high-impact transparent polypropylene special material prepared by the method according to any one of claims 1 to 9.