Modified ethylene-tetrafluoroethylene copolymer as well as preparation method and application thereof

By introducing fluoroalkyl modified monomers and fluoroallyl alkyl carbonates, the molar ratio of ethylene-tetrafluoroethylene copolymer is solved, and the problem of high temperature required for melt forming of copolymers at high temperatures is achieved, and low energy is achieved The effect of consumption and efficient processing is suitable for electrostatic spraying.

CN119039501APending Publication Date: 2024-11-29JUHUA GROUP TECH CENT +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411229647.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing ethylene-tetrafluoroethylene copolymers require high temperatures when melt-forming at high temperatures, resulting in increased production energy consumption and low tensile strength, making it difficult to meet the requirements of efficient processing and heat resistance.

Method used

The introduction of fluoroalkyl modified monomers and fluoroallyl alkyl carbonates is used to adjust the molar ratio of the copolymer, reduce the melting point and maintain good mechanical properties and thermal stability, which is suitable for electrostatic spraying applications.

Benefits of technology

It realizes a modified ethylene-tetrafluoroethylene copolymer with excellent leveling and thermal stability at lower temperatures, which is suitable for the field of electrostatic spraying, reduces production energy consumption and improves the efficiency of equipment use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005025699490000091
    Figure BDA0005025699490000091
  • Figure BDA0005025699490000101
    Figure BDA0005025699490000101
Patent Text Reader

Abstract

The invention belongs to the technical field of fluorine-containing polymers, and particularly relates to a modified ethylene-tetrafluoroethylene copolymer as well as a preparation method and application thereof. According to the modified ethylene-tetrafluoroethylene copolymer provided by the invention, a copolymerization unit comprises ethylene, tetrafluoroethylene, a fluoroalkyl modified monomer and fluoroallyl alkyl carbonate, and the fluoroalkyl modified monomer comprises at least one of perfluoroalkyl olefin or perfluoroalkyl vinyl ether. Wherein the molar ratio of the ethylene to the tetrafluoroethylene is (10-40): (90-60); the molar ratio of the fluoro alkyl modified monomer to the fluoro allyl alkyl carbonate is (80-50): (20-50), and the sum of the molar weight of the fluoro alkyl modified monomer and the molar weight of the fluoro allyl alkyl carbonate is 1-10 mol% of the modified ethylene-tetrafluoroethylene copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fluorine-containing polymers, and specifically relates to a modified ethylene-tetrafluoroethylene copolymer and a preparation method and application thereof. Background Art

[0002] Ethylene-tetrafluoroethylene (ETFE) copolymer powder coating has good melt processability, so it can be easily made into an anti-corrosion coating of any shape and without seams through electrostatic spraying, rotational molding, and fluidized bed dipping. The formed coating has excellent heat resistance, chemical resistance, weather resistance, and mechanical properties. Compared with other anti-corrosion lining materials such as PTFE and FEP, it has more balanced mechanical properties, good melt processability, good adhesion to the substrate, and almost no difference in corrosion resistance. The relatively high fluorine content of ETFE (more than 60%) effectively protects the carbon chain skeleton and provides good durability to the coating. The regularly arranged molecular structure gives it a certain degree of crystallinity, providing barrier properties for the coating and resisting the penetration of acids and alkalis. Therefore, ETFE copolymer powder has an irreplaceable position in the field of anti-corrosion.

[0003] In the powder coating process, the powder needs to be heated and baked after the powder coating is completed to make it melt, level and solidify. Therefore, the leveling property and high temperature color of the resin at high temperature are important factors affecting the spraying effect. In recent years, in order to improve production efficiency, reduce production costs and reduce energy consumption, ETFE resin must have very good leveling properties, can be melted and formed at a lower temperature, and the coating of the parts during the processing must be uniform, heat resistant and transparent.

[0004] Therefore, how to prepare modified ethylene-tetrafluoroethylene copolymers or compositions with good high-temperature stability, excellent processing properties and high transparency has received more and more attention. Summary of the invention

[0005] The present invention is based on the inventor's discovery and understanding of the following facts and problems:

[0006] CN117946346A discloses that a highly branched silicon-containing macromolecular third modified monomer unit is introduced to obtain an ethylene-tetrafluoroethylene modified copolymer, which greatly reduces the melting point of ETFE and mainly solves its thermal stress cracking problem. However, the tensile strength of the modified copolymer is relatively low, only reaching 4.9-5.7MPa.

[0007] CN104151754B adopts a two-stage method to prepare an ethylene-tetrafluoroethylene copolymer resin polymer with high melt fluidity and two melting points, which has high melt fluidity, good mechanical properties and heat resistance, and good yellowing performance, so it is suitable for high-speed extrusion molding and meets certain uses with high color requirements. However, due to the presence of a high melting point part (above 260°C) in the resin, a higher temperature is required to melt the resin during the molding process, and the processing temperature requirement is still very high, the production energy consumption increases, and the equipment requirements are also high.

[0008] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, an embodiment of the present invention provides a modified ethylene-tetrafluoroethylene copolymer, which has a low melting point, good leveling properties, good mechanical properties, excellent high temperature color, and can be applied to the field of electrostatic spraying.

[0009] The modified ethylene-tetrafluoroethylene copolymer of the embodiment of the present invention comprises copolymer units of ethylene, tetrafluoroethylene, a fluoroalkyl modified monomer and a fluoroallyl alkyl carbonate, wherein the fluoroalkyl modified monomer comprises at least one of a perfluoroalkyl olefin or a perfluoroalkyl vinyl ether; wherein:

[0010] The molar ratio of ethylene to tetrafluoroethylene is (10-40):(90-60);

[0011] The molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is (80-50):(20-50), and the sum of the molar amounts of the fluoroalkyl modified monomer and the fluoroallyl alkyl carbonate is 1-10 mol% of the modified ethylene-tetrafluoroethylene copolymer.

[0012] The advantages and technical effects brought by the modified ethylene-tetrafluoroethylene copolymer in the embodiment of the present invention are as follows: 1. In the embodiment of the present invention, a fluoroalkyl modified monomer is introduced into the copolymer, which destroys the regularity of the chain segment and can effectively reduce the melting point of the copolymer; 2. In the embodiment of the present invention, a fluoroallyl alkyl carbonate is introduced into the copolymer, and the fluoroallyl alkyl carbonate has excellent rigidity, which can enable the copolymer to maintain good mechanical properties and excellent thermal stability; 3. In the embodiment of the present invention, the molar ratio of ethylene to tetrafluoroethylene and the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is controlled, and the total molar percentage of the fluoroalkyl modified monomer and the fluoroallyl alkyl carbonate in the copolymer is controlled at the same time, which effectively reduces the melting point of the copolymer, makes the polymer have excellent leveling and thermal stability, and maintains good mechanical properties at the same time, and there is no yellowing phenomenon in high temperature testing, which is suitable for application in electrostatic spraying.

[0013] In some embodiments, the molar ratio of ethylene to tetrafluoroethylene is (20-30):(80-70).

[0014] In some embodiments, the molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is (70-60):(30-40).

[0015] In some embodiments, the perfluoroalkyl olefin includes at least one of perfluoropropylene, 1-perfluorobutene, perfluorobutylethylene, perfluorohexylethylene, and 1-perfluoropentene.

[0016] In some embodiments, the perfluoroalkyl vinyl ether includes at least one of perfluoroethyl vinyl ether, perfluoro-n-propyl vinyl ether, perfluoro-n-butyl vinyl ether, and perfluoroethyl perfluorovinyl ether.

[0017] In some embodiments, the fluoroallyl alkyl carbonate includes at least one of allyl perfluoropropyl carbonate or allyl perfluorobutyl carbonate.

[0018] The present invention also provides a method for preparing a modified ethylene-tetrafluoroethylene copolymer, which comprises the following steps:

[0019] (1) adding an organic solvent, a fluoroalkyl modified monomer, a fluoroallyl alkyl carbonate and a regulator into a reaction kettle under the protection of an inert gas;

[0020] (2) Ethylene and tetrafluoroethylene are added to a reaction kettle and heated simultaneously. After reaching the temperature and pressure required for the reaction, an initiator is added to react to obtain a modified ethylene-tetrafluoroethylene copolymer.

[0021] The advantages and technical effects brought by the preparation method of the modified ethylene-tetrafluoroethylene copolymer provided by the embodiment of the present invention are as follows: 1. In the method of the embodiment of the present invention, under nitrogen protection, the copolymer monomers are subjected to solution polymerization in the presence of a free radical initiator to achieve free radical copolymerization, so that the temperature is easy to control during the reaction, and polymerization is achieved quickly with fewer by-products, which is beneficial to improving the polymerization rate and conversion rate; 2. In the method of the embodiment of the present invention, the addition order of each polymerization monomer in the preparation process is set, which is beneficial to obtaining a copolymer with excellent comprehensive performance; 3. The method of the embodiment of the present invention is simple and efficient, has low requirements on equipment, and has low production energy consumption, which is convenient for promotion and application in industrial production.

[0022] In some embodiments, in step (1), the organic solvent includes at least one of hydrofluorocarbon compounds, chlorofluorocarbon compounds, and perfluoroether compounds;

[0023] And / or, the regulator includes at least one of cyclohexane, methanol, ethanol, ethyl acetate, tert-dodecyl mercaptan or n-dodecyl mercaptan.

[0024] In some embodiments, in step (2), the initiator comprises at least one of tert-butyl pivalate, azobisisobutyronitrile, cumene oxide, dicumyl peroxide, ammonium persulfate or potassium persulfate;

[0025] And / or, the temperature required for the reaction is 50-80° C., and the pressure required for the reaction is 1.0-2.0 MPa;

[0026] And / or, after the reaction is completed, the temperature and pressure are reduced to discharge the material, and the obtained material is washed and dried.

[0027] The embodiments of the present invention also provide the use of the modified ethylene-tetrafluoroethylene copolymer or the modified ethylene-tetrafluoroethylene copolymer prepared by the preparation method in electrostatic spraying. DETAILED DESCRIPTION

[0028] Embodiments of the present invention are described in detail below. The embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0029] The modified ethylene-tetrafluoroethylene copolymer of the embodiment of the present invention comprises copolymer units of ethylene, tetrafluoroethylene, a fluoroalkyl modified monomer and a fluoroallyl alkyl carbonate, wherein the fluoroalkyl modified monomer comprises at least one of a perfluoroalkyl olefin or a perfluoroalkyl vinyl ether; wherein:

[0030] The molar ratio of ethylene to tetrafluoroethylene is (10-40):(90-60);

[0031] The molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is (80-50):(20-50), and the sum of the molar amounts of the fluoroalkyl modified monomer and the fluoroallyl alkyl carbonate is 1-10 mol% of the modified ethylene-tetrafluoroethylene copolymer.

[0032] The modified ethylene-tetrafluoroethylene copolymer of the embodiment of the present invention introduces a fluoroalkyl modified monomer into the copolymer, destroys the regularity of the chain segment, and can effectively reduce the melting point of the copolymer; introduces a fluoroallyl alkyl carbonate into the copolymer, and the fluoroallyl alkyl carbonate has excellent rigidity, which can enable the copolymer to maintain good mechanical properties and excellent thermal stability; the molar ratio of ethylene to tetrafluoroethylene and the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is controlled, and the total molar percentage of the fluoroalkyl modified monomer and the fluoroallyl alkyl carbonate in the copolymer is controlled at the same time, which effectively reduces the melting point of the copolymer, enables the polymer to have excellent leveling and thermal stability, and maintains good mechanical properties, and has no yellowing phenomenon in high temperature testing, and is suitable for application in electrostatic spraying.

[0033] In some embodiments, preferably, the molar ratio of ethylene to tetrafluoroethylene is (20-30):(80-70).

[0034] In the embodiments of the present invention, the molar ratio of ethylene to tetrafluoroethylene is preferably selected, which is beneficial to lowering the melting point of the polymer and maintaining the tensile strength and elongation at break at a high level.

[0035] In some embodiments, preferably, the molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is (70-60):(30-40).

[0036] In the embodiments of the present invention, the molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is preferably selected, and the polymer has excellent mechanical properties, thermal stability, a relatively low melting point and good leveling properties.

[0037] In some embodiments, preferably, the perfluoroalkyl olefin includes at least one of perfluoropropylene, 1-perfluorobutene, perfluorobutylethylene, perfluorohexylethylene, and 1-perfluoropentene; the perfluoroalkyl vinyl ether includes at least one of perfluoroethyl vinyl ether, perfluoro-n-propyl vinyl ether, perfluoro-n-butyl vinyl ether, and perfluoroethyl perfluorovinyl ether. Further preferably, the fluoroalkyl modified monomer is perfluorobutylethylene.

[0038] In the embodiments of the present invention, perfluoroalkyl olefins and perfluoroalkyl vinyl ethers are preferred. Such substances have long branched chain structures and can more effectively destroy the regularity of the chain segments, thereby reducing the melting point of the copolymer.

[0039] In some embodiments, preferably, the fluoroallyl alkyl carbonate comprises at least one of allyl perfluoropropyl carbonate or allyl perfluorobutyl carbonate. Further preferably, the fluoroallyl alkyl carbonate is allyl perfluorobutyl carbonate.

[0040] The present invention also provides a method for preparing a modified ethylene-tetrafluoroethylene copolymer, which comprises the following steps:

[0041] (1) Under the protection of inert gas, an organic solvent, a fluoroalkyl modified monomer, a fluoroallyl alkyl carbonate and a regulator are added into a reaction kettle;

[0042] (2) Ethylene and tetrafluoroethylene are added to a reaction kettle and heated simultaneously. After reaching the temperature and pressure required for the reaction, an initiator is added to react to obtain a modified ethylene-tetrafluoroethylene copolymer.

[0043] The preparation method of the modified ethylene-tetrafluoroethylene copolymer provided in the embodiment of the present invention realizes free radical copolymerization by solution polymerization of the copolymer monomers in the presence of a free radical initiator under nitrogen protection, so that the temperature is easy to control during the reaction, the polymerization is realized quickly, and there are fewer by-products, which is beneficial to improving the polymerization rate and conversion rate; the preparation method sets the order of adding each polymerization monomer during the preparation process, which is beneficial to preparing a copolymer with excellent comprehensive performance; the preparation method is simple and efficient, has low requirements on equipment, low production energy consumption, and is easy to promote and apply in industrial production.

[0044] In some embodiments, preferably, in step (1), the organic solvent comprises at least one of hydrofluorocarbon compounds, chlorofluorocarbon compounds, and perfluoroether compounds;

[0045] And / or, the regulator includes at least one of cyclohexane, methanol, ethanol, ethyl acetate, tert-dodecyl mercaptan or n-dodecyl mercaptan.

[0046] Further preferably, the organic solvent includes at least one of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (HFE-347) or 2,3-dichlorooctafluorobutane, and the organic solvent accounts for 60-70% of the volume of the reactor.

[0047] In some embodiments, preferably, in the step (2), the initiator comprises at least one of tert-butyl pivalate, azobisisobutyronitrile, cumene oxide, dicumyl peroxide, ammonium persulfate or potassium persulfate;

[0048] And / or, the temperature required for the reaction is 50-80° C., and the pressure required for the reaction is 1.0-2.0 MPa;

[0049] And / or, after the reaction is completed, the temperature and pressure are reduced to discharge the material, and the obtained material is washed and dried.

[0050] In some embodiments, after the initiator is added for reaction, it is necessary to continuously add a mixed gas of ethylene and tetrafluoroethylene to maintain the reaction pressure to ensure that the reaction proceeds in the forward direction and that products are continuously produced. When the yield reaches the production requirement, the addition of ethylene and tetrafluoroethylene is stopped and the reaction is stopped. During the reaction, the amount of fluoroalkyl modified monomer, fluoroallyl alkyl carbonate, regulator or initiator is added according to actual needs and the set material ratio.

[0051] The embodiments of the present invention also provide the use of the modified ethylene-tetrafluoroethylene copolymer or the modified ethylene-tetrafluoroethylene copolymer prepared by the preparation method in electrostatic spraying.

[0052] The technical solution of the present invention is described in detail below in conjunction with specific embodiments.

[0053] Example 1

[0054] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10 ppm, and then 4500 g of HFE-347, 20 g of perfluorobutylethylene, 10 g of allyl perfluorobutyl carbonate, and 2 g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64° C., and a mixed gas of ethylene and tetrafluoroethylene in a molar percentage of 20:80 was introduced at the same time until the pressure reached 1.5 MPa.

[0055] (2) Add 0.5 g of tert-butyl peroxypivalate using an auxiliary pump to initiate the reaction. After the polymerization begins, continue to add the mixed monomer to maintain a stable polymerization pressure. When the amount of the added ethylene and tetrafluoroethylene mixed gas reaches 500 g, stop the reaction, cool down to recover the unreacted mixed monomer, empty and replace the reactor, discharge the material from the reactor discharge valve, and obtain 450 g of ethylene-tetrafluoroethylene copolymer resin by rotary evaporation and drying.

[0056] Example 2

[0057] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10ppm, and then 4500g of HFE-347, 15g of perfluoro-n-propyl vinyl ether, 10g of allyl perfluorobutyl carbonate, and 2g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene with a molar percentage of 15:85 was introduced until the pressure reached 1.5MPa.

[0058] (2) 0.5 g of tert-butyl peroxypivalate was added by an auxiliary pump to initiate the reaction. After the polymerization started, the mixed monomer was continuously added to maintain the polymerization pressure stable. When the amount of the added ethylene and tetrafluoroethylene mixed gas reached 500 g, the reaction was stopped, the temperature was lowered to recover the unreacted mixed monomer, the reactor was vented and replaced, and the material was discharged from the reactor discharge valve, and 421 g of ethylene-tetrafluoroethylene copolymer resin was obtained after rotary evaporation and drying.

[0059] Example 3

[0060] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10 ppm, and then 4500 g of HFE-347, 20 g of perfluorobutylethylene, 15 g of allyl perfluoropropyl carbonate, and 2 g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene in a molar percentage of 10:90 was introduced until the pressure reached 1.5 MPa.

[0061] (2) Add 0.5 g of tert-butyl peroxypivalate using an auxiliary pump to initiate the reaction. After the polymerization begins, continue to add the mixed monomer to maintain a stable polymerization pressure. When the amount of the added ethylene and tetrafluoroethylene mixed gas reaches 500 g, stop the reaction, cool down to recover the unreacted mixed monomer, empty and replace the reactor, discharge the material from the reactor discharge valve, and obtain 440 g of ethylene-tetrafluoroethylene copolymer resin by rotary evaporation and drying.

[0062] Example 4

[0063] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10 ppm, and then 5100 g of 2,3-dichlorooctafluorobutane, 20 g of perfluorobutylethylene, 10 g of allyl perfluorobutyl carbonate, and 2 g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 65°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene in a molar percentage of 20:80 was introduced until the pressure reached 1.4 MPa.

[0064] (2) Add 0.5 g of tert-butyl peroxypivalate using an auxiliary pump to initiate the reaction. After the polymerization begins, continue to add the mixed monomer to maintain a stable polymerization pressure. When the amount of the added ethylene and tetrafluoroethylene mixed gas reaches 500 g, stop the reaction, cool down to recover the unreacted mixed monomer, empty and replace the reactor, discharge the material from the reactor discharge valve, and obtain 450 g of ethylene-tetrafluoroethylene copolymer resin by rotary evaporation and drying.

[0065] Example 5

[0066] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10ppm, and then 5100g of 2,3-dichlorooctafluorobutane, 10g of perfluorobutylethylene, 6g of allyl perfluorobutyl carbonate, and 7g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 65°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene in a molar percentage of 15:85 was introduced until the pressure reached 1.4MPa.

[0067] (2) 0.5 g of tert-butyl peroxypivalate was added by an auxiliary pump to initiate the reaction. After the polymerization started, the mixed monomer was continuously added to maintain the polymerization pressure stable. When the amount of the added ethylene and tetrafluoroethylene mixed gas reached 500 g, the reaction was stopped, the temperature was lowered to recover the unreacted mixed monomer, the reactor was vented and replaced, and the material was discharged from the reactor discharge valve, and 478 g of ethylene-tetrafluoroethylene copolymer resin was obtained after rotary evaporation and drying.

[0068] Example 6

[0069] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10ppm, and then 5100g of 2,3-dichlorooctafluorobutane, 25g of perfluorobutylethylene, 15g of allyl perfluorobutyl carbonate, and 1g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 65°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene with a molar percentage of 15:85 was introduced until the pressure reached 1.6MPa.

[0070] (2) 0.7 g of tert-butyl peroxypivalate was added by an auxiliary pump to initiate the reaction. After the polymerization started, the mixed monomer was continuously added to maintain the polymerization pressure stable. When the amount of the added ethylene and tetrafluoroethylene mixed gas reached 480 g, the reaction was stopped, the temperature was lowered to recover the unreacted mixed monomer, the reactor was vented and replaced, and the material was discharged from the reactor discharge valve, and 402 g of ethylene-tetrafluoroethylene copolymer resin was obtained after rotary evaporation and drying.

[0071] Comparative Example 1

[0072] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10 ppm, and then 4500 g of HFE-347, 20 g of perfluorobutylethylene, 9 g of allyl perfluorobutyl carbonate, and 2 g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64° C., and a mixed gas of ethylene and tetrafluoroethylene in a molar percentage of 40:60 was introduced at the same time until the pressure reached 1.5 MPa.

[0073] (2) 0.5 g of tert-butyl peroxypivalate was added by an auxiliary pump to initiate the reaction. After the polymerization started, the mixed monomer was continuously added to maintain the polymerization pressure stable. When the amount of the added ethylene and tetrafluoroethylene mixed gas reached 500 g, the reaction was stopped, the temperature was lowered to recover the unreacted mixed monomer, the reactor was vented and replaced, and the material was discharged from the reactor discharge valve, and 409 g of ethylene-tetrafluoroethylene copolymer resin was obtained after rotary evaporation and drying.

[0074] Comparative Example 2

[0075] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10 ppm, and then 4500 g of HFE-347, 20 g of perfluorobutylethylene, 9 g of allyl perfluorobutyl carbonate, and 2 g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene in a molar percentage of 8:92 was introduced until the pressure reached 1.5 MPa.

[0076] (2) Add 0.5 g of tert-butyl peroxypivalate using an auxiliary pump to initiate the reaction. After the polymerization begins, continue to add the mixed monomer to maintain the polymerization pressure stable. When the amount of the added ethylene and tetrafluoroethylene mixed gas reaches 500 g, stop the reaction, cool down to recover the unreacted mixed monomer, empty and replace the reactor, discharge the material from the reactor discharge valve, and obtain 456 g of ethylene-tetrafluoroethylene copolymer resin by rotary evaporation and drying.

[0077] Comparative Example 3

[0078] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10ppm, and then 4500g of HFE-347, 40g of perfluorobutylethylene, 10g of allyl perfluorobutyl carbonate, and 1g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene with a molar percentage of 15:85 was introduced until the pressure reached 1.5MPa.

[0079] (2) 0.5 g of tert-butyl peroxypivalate was added by an auxiliary pump to initiate the reaction. After the polymerization started, the mixed monomer was continuously added to maintain the polymerization pressure stable. When the amount of the added ethylene and tetrafluoroethylene mixed gas reached 500 g, the reaction was stopped, the temperature was lowered to recover the unreacted mixed monomer, the reactor was vented and replaced, and the material was discharged from the reactor discharge valve, and 390 g of ethylene-tetrafluoroethylene copolymer resin was obtained after rotary evaporation and drying.

[0080] Comparative Example 4

[0081] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10ppm, and then 4500g of HFE-347, 8g of perfluorobutylethylene, 3g of allyl perfluorobutyl carbonate, and 2g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64°C, and a mixed gas of ethylene and tetrafluoroethylene in a molar percentage of 20:80 was introduced until the pressure reached 1.5MPa.

[0082] (2) Add 0.5 g of tert-butyl peroxypivalate using an auxiliary pump to initiate the reaction. After the polymerization begins, continue to add the mixed monomer to maintain a stable polymerization pressure. When the amount of the added ethylene and tetrafluoroethylene mixed gas reaches 500 g, stop the reaction, cool down to recover the unreacted mixed monomer, empty and replace the reactor, discharge the material from the reactor discharge valve, and obtain 450 g of ethylene-tetrafluoroethylene copolymer resin by rotary evaporation and drying.

[0083] Comparative Example 5

[0084] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10ppm, and then 4500g of HFE-347, 35g of perfluorobutylethylene, 3g of allyl perfluorobutyl carbonate, and 2g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene with a molar percentage of 20:80 was introduced until the pressure reached 1.5MPa.

[0085] (2) 0.5 g of tert-butyl peroxypivalate was added by an auxiliary pump to initiate the reaction. After the polymerization started, the mixed monomer was continuously added to maintain the polymerization pressure stable. When the amount of the added ethylene and tetrafluoroethylene mixed gas reached 500 g, the reaction was stopped, the temperature was lowered to recover the unreacted mixed monomer, the reactor was vented and replaced, and the material was discharged from the reactor discharge valve, and 423 g of ethylene-tetrafluoroethylene copolymer resin was obtained after rotary evaporation and drying.

[0086] Comparative Example 6

[0087] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10ppm, and then 4500g of HFE-347, 20g of perfluorobutylethylene, 20g of allyl perfluorobutyl carbonate, and 1.5g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene with a molar percentage of 20:80 was introduced until the pressure reached 1.5MPa.

[0088] (2) 0.5 g of tert-butyl peroxypivalate was added by an auxiliary pump to initiate the reaction. After the polymerization started, the mixed monomer was continuously added to maintain the polymerization pressure stable. When the amount of the added ethylene and tetrafluoroethylene mixed gas reached 500 g, the reaction was stopped, the temperature was lowered to recover the unreacted mixed monomer, the reactor was vented and replaced, and the material was discharged from the reactor discharge valve, and 466 g of ethylene-tetrafluoroethylene copolymer resin was obtained after rotary evaporation and drying.

[0089] Comparative Example 7

[0090] (1) A 5L vertical stainless steel polymerization kettle equipped with a stirring paddle was first filled with nitrogen and evacuated for multiple replacements until the oxygen content was less than 10ppm, and then 4500g of HFE-347, 20g of perfluorobutylethylene, and 2g of cyclohexane were added. Stirring was started and the temperature of the polymerization kettle was raised to 64°C. At the same time, a mixed gas of ethylene and tetrafluoroethylene in a molar percentage of 20:80 was introduced until the pressure reached 1.5MPa.

[0091] (2) Add 0.5 g of tert-butyl peroxypivalate using an auxiliary pump to initiate the reaction. After the polymerization begins, continue to add the mixed monomer to maintain a stable polymerization pressure. When the amount of the added ethylene and tetrafluoroethylene mixed gas reaches 500 g, stop the reaction, cool down to recover the unreacted mixed monomer, empty and replace the reactor, discharge the material from the reactor discharge valve, and obtain 473 g of ethylene-tetrafluoroethylene copolymer resin by rotary evaporation and drying.

[0092] The contents and molar ratios of the monomers in the ethylene-tetrafluoroethylene copolymers prepared in Examples 1 to 6 and Comparative Examples 1 to 7 are shown in Table 1. The ethylene-tetrafluoroethylene copolymer resins prepared in Examples 1 to 6 and Comparative Examples 1 to 7 were tested, and the test results are shown in Table 2. The relevant test methods are shown as follows:

[0093] (1) Determination of copolymer composition (mol%)

[0094] The composition of the copolymer was calculated from the intensity ratio of specific groups measured by Fourier transform infrared spectroscopy.

[0095] (2) Melting point test (T m ,℃)

[0096] 5-10 mg of the copolymer was taken and placed in a sample cell, and the temperature was raised from 100°C to 300°C at a rate of 10°C / min, and the changes in the curve were recorded. The DSC instrument was DCS702 from Seiko Instruments Co., Ltd. of Japan.

[0097] (3) Melt index measurement (MFI, g / 10min)

[0098] The melt index test was conducted according to the international standard ASTM-3159. The test load was 5kg, the temperature was 297°C, and the instrument used was the MF30 melt index tester from Ceast, Italy. (Note: The melt index of the resin is controlled between 20 and 30 g / 10 min according to the needs of electrostatic spraying processing)

[0099] (4) Thermal stability test (T 5wt% , ℃)

[0100] Using a thermogravimetric analyzer (Seiko Instruments Co., Ltd., TG / DTA6300), about 3-5 mg of copolymer sample was heated from room temperature to 500°C at a rate of 10°C / min in an air atmosphere, and the temperature at which the weight loss was 5 wt% was taken to measure the thermal stability of the polymer. 5wt% <370℃ indicates poor heat resistance.

[0101] (5) Mechanical properties test

[0102] The compression molding technology was used to prepare the tensile test specimens, and the mechanical properties test was carried out in accordance with GB / T 1040.1-2006.

[0103] (6) High temperature color test

[0104] Put about 30g of ETFE resin powder into tin foil, heat it in a 300℃ oven for 2h, take it out and cool it to room temperature, and observe the color change of the sample.

[0105] Table 1

[0106]

[0107] Table 2

[0108]

[0109] It can be seen from the data in Table 1 and Table 2 that the modified ethylene-tetrafluoroethylene copolymers prepared in Examples 1 to 6 simultaneously satisfy the following conditions: the sum of the fluoroalkyl modified monomer and the fluoroallyl alkyl carbonate is 1 to 10 mol% of the modified ethylene-tetrafluoroethylene copolymer, the molar ratio of ethylene to tetrafluoroethylene is (10 to 40):(90 to 60), and the molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is (80 to 50):(20 to 50). The prepared polymer has good mechanical properties, thermal stability and leveling properties, a melting point of less than 230°C, and excellent high temperature color, and is suitable for application in the field of electrostatic spraying.

[0110] In the copolymer of Comparative Example 1, the ratio of ethylene to tetrafluoroethylene is 44:56, and too much ethylene comonomer is introduced. Although the mechanical properties and thermal stability are improved, the melting point of the copolymer is greatly increased, and the copolymer turns yellow after 2 hours at 300°C.

[0111] In the copolymer of Comparative Example 2, the ratio of ethylene to tetrafluoroethylene is 9:91, and too much tetrafluoroethylene comonomer is introduced. Although the thermal stability is improved, the melting point of the copolymer is as high as 268° C., and the copolymer turns yellow after 2 hours at 300° C.

[0112] In the copolymer of Comparative Example 3, the total amount of fluoroalkyl modified monomer and allyl alkyl carbonate introduced is too much. Although the melting point of the copolymer is reduced, the mechanical properties and thermal stability are greatly reduced, and yellowing occurs in the high temperature color test.

[0113] In the copolymer of Comparative Example 4, the total amount of fluoroalkyl modified monomer and allyl alkyl carbonate introduced is too small. Although the polymer can have good thermal stability and mechanical properties, its melting point is increased, and yellowing occurs in the high temperature color test, and the high temperature yellowing resistance is poor.

[0114] In the copolymer in Comparative Example 5, the molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is 85:15, and too much fluoroalkyl modified monomer is introduced; the leveling performance of the polymer is slightly improved, but the thermal weight loss temperature is reduced to 310°C, the tensile strength is reduced to 40 MPa, the elongation at break is reduced to 330%, and yellowing occurs in the high temperature color test, and the high temperature yellowing resistance is poor.

[0115] In the copolymer of Comparative Example 6, the molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is 43:57. Too much fluoroallyl alkyl carbonate is introduced. Although the mechanical properties, thermal stability, melting point and leveling properties of the polymer are not significantly affected, the high temperature yellowing resistance is poor.

[0116] In the copolymer of Comparative Example 7, no fluoroallyl alkyl carbonate was introduced. Although the melting point remained at a low level, the leveling performance was excellent, and the thermal stability was good, the tensile strength was reduced to 39.3 MPa, the elongation at break was reduced to 220%, and yellowing occurred in the high temperature color test.

[0117] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0118] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. A modified ethylene-tetrafluoroethylene copolymer, characterized in that: The copolymer units include ethylene, tetrafluoroethylene, a fluoroalkyl modified monomer and a fluoroallyl alkyl carbonate, wherein the fluoroalkyl modified monomer includes at least one of a perfluoroalkyl olefin or a perfluoroalkyl vinyl ether; wherein, The molar ratio of ethylene to tetrafluoroethylene is (10-40):(90-60); The molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is (80-50):(20-50), and the sum of the molar amounts of the fluoroalkyl modified monomer and the fluoroallyl alkyl carbonate is 1-10 mol% of the modified ethylene-tetrafluoroethylene copolymer.

2. The modified ethylene-tetrafluoroethylene copolymer according to claim 1, characterized in that The molar ratio of ethylene to tetrafluoroethylene is (20-30):(80-70).

3. The modified ethylene-tetrafluoroethylene copolymer according to claim 1, characterized in that The molar ratio of the fluoroalkyl modified monomer to the fluoroallyl alkyl carbonate is (70-60):(30-40).

4. The modified ethylene-tetrafluoroethylene copolymer according to claim 1, characterized in that The perfluoroalkyl olefin includes at least one of perfluoropropylene, 1-perfluorobutene, perfluorobutylethylene, perfluorohexylethylene, and 1-perfluoropentene.

5. The modified ethylene-tetrafluoroethylene copolymer according to claim 1, characterized in that: The perfluoroalkyl vinyl ether includes at least one of perfluoroethyl vinyl ether, perfluoro-n-propyl vinyl ether, perfluoro-n-butyl vinyl ether and perfluoroethyl perfluorovinyl ether.

6. The modified ethylene-tetrafluoroethylene copolymer according to claim 1, characterized in that The fluoroallyl alkyl carbonate includes at least one of allyl perfluoropropyl carbonate or allyl perfluorobutyl carbonate.

7. The method for preparing a modified ethylene-tetrafluoroethylene copolymer according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) adding an organic solvent, a fluoroalkyl modified monomer, a fluoroallyl alkyl carbonate and a regulator into a reaction kettle under the protection of an inert gas; (2) Ethylene and tetrafluoroethylene are added to a reaction kettle and heated simultaneously. After reaching the temperature and pressure required for the reaction, an initiator is added to react to obtain a modified ethylene-tetrafluoroethylene copolymer.

8. The method for preparing the modified ethylene-tetrafluoroethylene copolymer according to claim 7, characterized in that: In the step (1), the organic solvent comprises at least one of a hydrofluorocarbon compound, a chlorofluorocarbon compound or a perfluoroether compound; And / or, the regulator includes at least one of cyclohexane, methanol, ethanol, ethyl acetate, tert-dodecyl mercaptan or n-dodecyl mercaptan.

9. The method for preparing the modified ethylene-tetrafluoroethylene copolymer according to claim 7, characterized in that: In the step (2), the initiator comprises at least one of tert-butyl pivalate, azobisisobutyronitrile, cumene oxide, dicumyl peroxide, ammonium persulfate or potassium persulfate; And / or, the temperature required for the reaction is 50-80° C., and the pressure required for the reaction is 1.0-2.0 MPa; And / or, after the reaction is completed, the temperature and pressure are reduced to discharge the material, and the obtained material is washed and dried.

10. Use of the modified ethylene-tetrafluoroethylene copolymer according to any one of claims 1 to 6 or the modified ethylene-tetrafluoroethylene copolymer prepared by the preparation method according to any one of claims 7 to 9 in electrostatic spraying.

Citation Information

Cited By

  • Modified PTFE (Polytetrafluoroethylene) material as well as preparation method and application thereof in airbag pump

    CN121045718A