Method for proportionally and selectively recovering gallium, indium and selenium from flexible copper-gallium-indium-selenium thin-film solar cell leachate

By using the temperature-sensitive multi-template intelligent imprinted polymer prepared by RAFT in copper gallium indium selenium thin-film solar cell leaching solution for adsorption/desorption, the problem of gallium, indium and selenium elements is solved, and efficient and low-cost proportional recycling is achieved. , reduces environmental impact.

CN119039532AInactive Publication Date: 2024-11-29LANZHOU UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202411457812.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently recover and reuse gallium, indium and selenium elements in copper gallium indium selenium thin-film solar cells, and its environmental impact is great, especially after the post-decommissioning recovery process.

Method used

Reversible addition-break chain transfer polymerization (RAFT) is used to prepare temperature-sensitive multi-template intelligent imprinted polymer, and the multi-template intelligent imprinted polymer is synthesized by solution polymerization method, and the copper gallium indium selenium thin-film solar cell leaching liquid is used to utilize its adsorption/desorption characteristics. Selective recycling of gallium, indium and selenium elements.

Benefits of technology

It realizes proportional selective recycling of low-energy consumption and low-cost gallium, indium and selenium elements under room temperature conditions, improves recycling efficiency and reduces process costs, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039532A_ABST
    Figure CN119039532A_ABST
Patent Text Reader

Abstract

The invention discloses a method for proportionally and selectively recovering gallium, indium and selenium from a flexible copper gallium indium selenium thin film solar cell leachate, which comprises the following steps: preparing a linear thermo-sensitive polymer poly N, N-diethylacrylamide (PDEA) by adopting reversible addition-fragmentation chain transfer polymerization (RAFT); synthesizing a temperature-sensitive block PDEA-b-P (DEA-co-AM) from the synthesized poly (N, N-diethylacrylamide) (PDEA) serving as an RAFT (reversible addition fragmentation chain transfer) reagent and acrylamide (AM); a temperature-sensitive block is introduced through a solution polymerization method to synthesize a multi-template intelligent imprinted polymer (GIS-SIIP); and then eluting template ions from the dried and crushed imprinted polymer (GIS-SIIP) to obtain the adsorbent. And finally, carrying out primary adsorption / desorption circulation on the gallium-indium-selenium thin-film solar cell leachate by using an adsorbent to obtain a desorption recovery solution in which the amount of substances of gallium, indium and selenium ions is in a certain proportion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of precious metal recovery, and in particular to a preparation method for recovering gallium, indium and selenium in proportion from a copper gallium indium selenium thin-film solar cell leachate. Background Art

[0002] The absorption layer of copper gallium indium selenide (CIGS) thin-film solar cells contains four elements: copper, indium, gallium, and selenium. Among them, the global selenium resources are relatively small, and most of them are associated with sulfide minerals. The enrichment of selenium in industry mainly comes from copper anode mud. High-purity selenium is regarded as a key material in metallurgy, semiconductors and other fields. Indium and gallium are globally recognized strategic elements as scattered metal elements. Indium and gallium do not have their own independent deposits, but are produced as by-products of the metallurgical industry. Indium and gallium mainly come from the hydrometallurgical zinc industry and the aluminum extraction industry. The abundance of indium and gallium in these minerals is low, ranging from tens to hundreds of parts per million, which means that the extraction and enrichment process is troublesome. Therefore, the global production of native indium and gallium is affected by their native minerals. In addition, in terms of environmental impact, studies have shown that CIGS ranks second only to cadmium telluride in global warming potential and other impact categories. Overall, CIGS shows relatively positive environmental impact results. However, since CIGS is in the early stages of commercialization and the current commercial CIGS has not yet reached the retirement deadline, the CIGS recycling process has received less environmental assessment. The environmental impact of recycling CIGS after decommissioning is worrying, so it is necessary to consider the recycling and reuse of valuable metal elements in scrap CIGS. Summary of the invention

[0003] The present invention aims to provide a short-process, high-efficiency method for selectively recovering gallium, indium and selenium in proportion from a leachate of a flexible copper-gallium-indium-selenium thin-film solar cell.

[0004] To achieve the above object, the present invention adopts the following technical solutions: First, the linear thermosensitive polymer poly (N,N-diethylacrylamide) (PDEA) was prepared by reversible addition-fragmentation chain transfer polymerization (RAFT); the synthesized poly (N,N-diethylacrylamide) (PDEA) was used as a RAFT agent to synthesize the thermosensitive block PDEA-bP (DEA-co-AM) with acrylamide (AM); the thermosensitive block was introduced by solution polymerization to synthesize a multi-template intelligent imprinted polymer (GIS-SIIP); then the template ions were eluted from the dried and crushed imprinted polymer (GIS-SIIP) to obtain the adsorbent; finally, the adsorbent was used to perform an adsorption / desorption cycle on the leaching solution of gallium indium selenide thin film solar cells to obtain a desorption recovery solution in which the amounts of gallium, indium and selenium ions were in a certain proportion.

[0005] The specific steps are as follows: 1) PDEA synthesis Azobisisobutyronitrile, 2-(dodecyl trithiocarbonate)-2-methylpropionic acid and N,N-diethylacrylamide are dissolved in ethyl acetate, mixed evenly, and sealed after nitrogen is passed for 15-20 minutes. The mixture is stirred in an oil bath at 60-80°C for 30-40 hours. After the reaction is completed, ethyl acetate is used as a solvent and n-hexane is used as a precipitant. The mixture is dissolved and precipitated three times to obtain poly (N,N-diethylacrylamide, PDEA). The molar ratio of azobisisobutyronitrile, 2-(dodecyl trithiocarbonate)-2-methylpropionic acid and N,N-diethylacrylamide is 1:(15-25):(950-1050). The preferred molar ratio is 1:20:1000.

[0006] 2) Synthesis of thermosensitive block of PDEA-bP(DEA-co-AM) Azobisisobutyronitrile, PDEA, acrylamide and N,N-diethylacrylamide were dissolved in N,N-dimethylformamide, mixed evenly, and sealed after nitrogen was passed for 15-20 minutes. The mixture was stirred in an oil bath at 60-80°C for 30-40 hours. Ethyl acetate was used as solvent and n-hexane was used as precipitant. The mixture was dissolved and precipitated three times. The mixture was taken out and placed in a vacuum drying oven to a constant weight, thereby obtaining a thermosensitive block [poly (N,N-diethylacrylamide-g-poly (N,N-diethylacrylamide-g-acrylamide)], which was recorded as PDEA-bP (DEA-co-AM). The molar ratio of azobisisobutyronitrile, PDEA and acrylamide is 1:(15-20):(950-1050), preferably 1:20:1000; the molar ratio of N,N-diethylacrylamide to acrylamide is 1:1.5-1:2.5, preferably 1:2.

[0007] 3) GIS-SIIP synthesis PDEA-bP (DEA-co-AM), acrylamide, acrylic acid and template ions were dissolved in a mixed solution of methanol and water. After self-assembly in a water bath at 30-35°C for 1-2 hours, a crosslinking agent N,N-methylenebisacrylamide was added, nitrogen was passed through for 15-20 minutes and then sealed. The redox initiation system AP-TEMED was injected into the system with a syringe and then sealed. After initiating polymerization at 30-40°C for 20-25 hours, the system was taken out and placed in a vacuum drying oven to be dried to constant weight to obtain GIS-SIIP. The mass ratio of PDEA-bP to acrylic acid is 1:5-1:20, the molar ratio of acrylamide to acrylic acid is 1:2-2:1, and the molar ratio of acrylic acid to N,N-methylenebisacrylamide is 1:5-1:7.

[0008] The template ion is a mixed ion system composed of gallium, indium and selenium ions in a molar ratio of 1:4:8, and the amount of template ions added accounts for 30% to 40% of the molar amount of acrylic acid. Specifically, the template ion solution is obtained by mixing equal volumes of 0.0246mmol / mL selenic acid solution, 0.0124mmol / mL indium trichloride solution and 0.0030mmol / mL gallium trichloride solution.

[0009] The AP-TEMED redox initiation system is formed by mixing equal volumes of an ammonium persulfate solution and an N,N,N,N-tetramethylethylenediamine solution at a molar concentration ratio of 1:2.

[0010] 4) Adsorbent preparation The dried GIS-SIIP was crushed, and the particles of 30-100 mesh were sieved with a sieve and stored. The particles were put into a 200-mesh filter bag and placed in a Soxhlet extractor. The template ions were eluted with analytically pure anhydrous ethanol as the eluent. The corresponding template ion concentration in the etching solution was determined by ICP-AES. When the test value was lower than 0.02 μg / mL, the elution was stopped. The filter bag was then rinsed alternately with methanol and water until the solution was neutral, and dried in a vacuum drying oven to constant weight to obtain the adsorbent.

[0011] 5) Ion adsorption / desorption The adsorbent is placed in the leachate of a flexible copper gallium indium selenide thin film solar cell for adsorption, the adsorption temperature is 35°C, and the adsorption time is 120 min; after the adsorption is completed, the adsorbent is placed in a mixed solution containing 0.1 mol / L HCl and 0.3 mol / L thiourea for desorption, the desorption temperature is 25°C, and the desorption time is 300 min; thus, a desorption solution of gallium, indium, and selenium elements recovered in proportion is obtained.

[0012] The leachate of the flexible copper gallium indium selenide thin film solar cell is obtained by first mechanically stripping the outer protective film and substrate of the copper gallium indium selenide thin film solar cell, then cleaning the photovoltaic component after stripping the protective layer with dimethyl sulfoxide, and finally washing the residual dimethyl sulfoxide with ethanol and water for pretreatment.

[0013] The pretreatment process is as follows: hydrochloric acid (HCl) is used as the medium in the leaching process, with 5 vol% hydrogen peroxide (H 2 O 2 ) 5 mol / L HCl solution was used as the leaching solution, with a solid-liquid ratio of 5 g / L, a leaching temperature of 35~45°C, and a leaching time of 1~2 h.

[0014] The proportional recovery means that except for gallium, indium and selenium, the content of other interfering elements in the analytical solution accounts for less than 10%.

[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention makes full use of the characteristics of physical adsorption, which is safe, green and easy to desorb, and combines the selectivity of ion imprinting technology to achieve specific selective recovery of gallium, indium and selenium elements in the leachate of flexible copper gallium indium selenide thin film solar cells; 2. The leaching, adsorption and recovery processes adopted by the present invention are all carried out at a temperature close to room temperature, so that the entire process has the advantages of green, low energy consumption and low cost; 3. The present invention introduces a temperature-sensitive block [poly (N,N-diethylacrylamide-g-poly (N,N-diethylacrylamide-g-acrylamide)], denoted as PDEA-bP (DEA-co-AM). The adsorption / desorption effect of ion-imprinted polymers is achieved by intelligently controlling the temperature, and the integrity of the imprinted holes is ensured during the adsorption process, while the desorption efficiency is improved, thereby increasing the recovery efficiency; 4. The present invention verifies that the amount of the template ion substance is related to the ratio of the amount of the adsorbed / analyzed target ion substance, making the recovery process more potentially applicable; 5. The present invention not only achieves the separation and enrichment of valuable elements gallium, indium and selenium in the leachate of waste flexible copper gallium indium selenide thin film solar cells, but also the ratio of the amount of gallium, indium and selenium ions in the desorption solution is close to the ratio of the amount of the corresponding template ion substances added, thereby achieving the effect of proportional selective recovery. At the same time, since the synthesized multi-template intelligent imprinted polymer can be reused many times and can be adsorbed and desorbed by temperature control, the result of reducing costs and improving efficiency is achieved, which is conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The figure is a flow chart for the preparation of the temperature-sensitive multi-template intelligent imprinting polymer GIS-SIIP in the present invention.

[0017] Figure 2 FTIR spectra of PDEA, P(DEA-co-AM) and PDEA-bP(DEA-co-AM) obtained in Example 1 of the present invention.

[0018] Figure 3 PDEA-bP(DEA-co-AM) prepared in Example 1 of the present invention 1 H NMR spectrum.

[0019] Figure 4 SEM images of the temperature-sensitive multi-template smart imprinted polymer (left) and the non-imprinted polymer (right) prepared in Example 1 of the present invention.

[0020] Figure 5The adsorption kinetic curves of the adsorbent 1 prepared in Example 1 of the present invention for a) gallium ions, b) indium ions, and c) selenate ions at 25°C, 35°C and 45°C.

[0021] Figure 6 Desorption kinetic curves of adsorbent 1 prepared in Example 1 of the present invention for a) gallium ions, b) indium ions, and c) selenate ions at 25°C, 35°C and 45°C.

[0022] Figure 7 This is a diagram of the reusability of adsorbent 1 obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0023] The present invention is further explained below with reference to specific embodiments.

[0024] according to Figure 1 The process shown is used to synthesize the temperature-sensitive multi-template intelligent imprinting polymer GIS-SIIP in the following three examples.

[0025] Example 1 Weigh 0.006g of azobisisobutyronitrile, 0.258g of 2-(dodecyl trithiocarbonate)-2-methylpropionic acid (RAFT agent) and 4.54g of N,N-diethylacrylamide (DEA), dissolve them completely in a 25mL test tube with 9.423g of ethyl acetate, mix them evenly, pass 99.999% pure nitrogen gas at room temperature for 15min, seal them, and stir them in a 70℃ oil bath for 36h. After the reaction, use ethyl acetate as solvent and n-hexane as precipitant to dissolve and precipitate the initial product three times to obtain poly N,N-diethylacrylamide (PDEA).

[0026] 0.003g of azobisisobutyronitrile, 1.3104g of poly N,N-diethylacrylamide (PDEA) and 0.6486g of acrylamide were weighed and completely dissolved in a 25mL test tube with 2.6804g of N,N-dimethylformamide, and then 0.4972g of N,N-diethylacrylamide (DEA) was added and mixed evenly. After nitrogen with a purity of 99.999% was introduced at room temperature for 15min, the mixture was sealed and stirred in an oil bath at 70℃ for 36h. A mixed solvent of ethyl acetate and n-hexane with a volume ratio of 1:4 was used as a precipitant, and three dissolutions and three precipitations were performed. Subsequently, the mixture was placed in a vacuum oven at 40℃ until constant weight was obtained, and the temperature-sensitive block [poly N,N-diethylacrylamide-g-poly(N,N-diethylacrylamide-g-acrylamide)] was obtained, which was recorded as PDEA-bP(DEA-co-AM).

[0027] As a comparison, the synthesis steps of P(DEA-co-AM) are given: 0.003g of azobisisobutyronitrile and 0.6486g of acrylamide are weighed and completely dissolved in a 25mL test tube with 2.6804g of N,N-dimethylformamide, and then 0.4972g of N,N-diethylacrylamide (DEA) is added, mixed evenly, nitrogen with a purity of 99.999% is introduced at room temperature for 15 minutes, and then sealed, and stirred in a 70°C oil bath for 36 hours. A mixed solvent of ethyl acetate and n-hexane with a volume ratio of 1:4 is used as a precipitant, and three dissolutions and three precipitations are performed. Subsequently, it is placed in a vacuum oven at 40°C until constant weight is obtained, and a random copolymer [poly(N,N-diethylacrylamide-g-acrylamide)] is obtained, which is recorded as P(DEA-co-AM).

[0028] Weigh 0.1 g of the thermosensitive block, 0.56 g of acrylamide, 0.5 g of acrylic acid and 0.2 mmol of template ions (0.123 mmol of SeO 4 2- , 0.062mmolIn 3+ and 0.015mmol of Ga 3+ ) was dissolved in a mixed solvent of water and methanol with a volume ratio of 1:2, and self-assembled for 1 hour in a constant temperature water bath at a temperature of 33°C and a magnetic stirring speed of 150 r / min. 6g of N,N-methylenebisacrylamide was added and stirred until completely dissolved. Nitrogen with a purity of 99.999% was introduced at room temperature for 15 minutes and then sealed to form a solution system. The same volume of ammonium persulfate solution with a molar volume concentration of 4.483mmol / L and N,N,N,N-tetramethylethylenediamine solution with a molar volume concentration of 8.964mmol / L were taken and mixed to form an AP-TEMED redox initiator system solution. The redox initiator system AP-TEMED was injected into the solution system with a syringe and then sealed. After initiating polymerization at 35°C, the solution was taken out and placed in a vacuum drying oven to dry to constant weight to obtain a temperature-sensitive multi-template intelligent imprinted polymer GIS-SIIP. The preparation of the non-ionic imprinted polymer (GIS-NSIIP) was the same as above except that the template ion was not added.

[0029] The dried polymer was crushed by a pulverizer, and 30-100 mesh particles were sieved with a sieve and stored, and then placed in a 200 mesh filter bag (7.6×50 mm), and placed in a Soxhlet extractor to elute the template ions with anhydrous ethanol, and the corresponding template ion concentration in the etching solution was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES) analysis technology. When the test value was lower than 0.02 μg / mL, the elution was stopped, and then the filter bag was alternately rinsed with methanol and water until the solution was neutral, and placed at 45°C for vacuum drying to constant weight. After drying, adsorbent 1 was obtained.

[0030] Example 2 Weigh 0.002g of azobisisobutyronitrile, 0.086g of 2-(dodecyl trithiocarbonate)-2-methylpropionic acid (RAFT agent) and 1.513g of N,N-diethylacrylamide (DEA), dissolve them completely in a 25mL test tube with 3.141g of ethyl acetate, mix them evenly, pass 99.999% pure nitrogen gas at room temperature for 15min, seal them, and stir them in a 70℃ oil bath for 36h. After the reaction, use ethyl acetate as solvent and n-hexane as precipitant to dissolve and precipitate the initial product three times to obtain poly N,N-diethylacrylamide (PDEA).

[0031] 0.006g of azobisisobutyronitrile, 2.621g of poly N,N-diethylacrylamide (PDEA) and 1.2972g of acrylamide were weighed and completely dissolved in a 25mL test tube with 5.3608g of N,N-dimethylformamide, and then 0.9944g of N,N-diethylacrylamide (DEA) was added and mixed evenly. After nitrogen with a purity of 99.999% was introduced at room temperature for 15min, the mixture was sealed and stirred in an oil bath at 70℃ for 36h. A mixed solvent of ethyl acetate and n-hexane with a volume ratio of 1:4 was used as a precipitant, and three dissolutions and three precipitations were performed. Subsequently, the mixture was placed in a vacuum oven at 40℃ until constant weight was obtained, and the temperature-sensitive block [poly N,N-diethylacrylamide-g-poly(N,N-diethylacrylamide-g-acrylamide)] was obtained, which was recorded as PDEA-bP(DEA-co-AM).

[0032] Weigh 0.05 g of the thermosensitive block, 0.56 g of acrylamide, 1.0 g of acrylic acid and 0.4 mmol of template ions (0.246 mmol of SeO 4 2- , 0.124mmol In 3+ and 0.030mmol of Ga 3+ ) was dissolved in a mixed solvent of water and methanol with a volume ratio of 1:2, and self-assembled for 1 hour in a constant temperature water bath at a temperature of 33°C and a magnetic stirring speed of 150 r / min. 7g of N,N-methylenebisacrylamide was added and stirred until completely dissolved. Nitrogen with a purity of 99.999% was introduced at room temperature for 15 minutes and then sealed to form a solution system. Take the same volume of ammonium persulfate solution with a molar volume concentration of 4.483mmol / L and N,N,N,N-tetramethylethylenediamine solution with a molar volume concentration of 8.964mmol / L, and mix them to form an AP-TEMED redox initiator system solution. The redox initiator system AP-TEMED was injected into the solution system with a syringe and then sealed. After initiating polymerization at 35°C, take it out and place it in a vacuum drying oven to dry to constant weight to obtain the temperature-sensitive multi-template intelligent imprinting polymer GIS-SIIP.

[0033] The dried polymer was crushed by a multifunctional pulverizer, and 30-100 mesh particles were sieved with a sieve and stored, and then placed in a 200 mesh filter bag (7.6×50 mm), and placed in a Soxhlet extractor to elute the template ions with anhydrous ethanol, and the corresponding template ion concentration in the etching solution was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES) analysis technology. When the test value was lower than 0.02 μg / mL, the elution was stopped, and then the filter bag was alternately rinsed with methanol and water until the solution was neutral, and then placed at 45°C for vacuum drying to constant weight. After drying, adsorbent 2 was obtained.

[0034] Example 3 Weigh 0.004g of azobisisobutyronitrile, 0.172g of 2-(dodecyl trithiocarbonate)-2-methylpropionic acid (RAFT agent) and 3.027g of N,N-diethylacrylamide (DEA), dissolve them completely in a 25mL test tube with 6.282g of ethyl acetate, mix them evenly, pass 99.999% pure nitrogen gas at room temperature for 15min, seal them, and stir them in a 70℃ oil bath for 36h. After the reaction, use ethyl acetate as solvent and n-hexane as precipitant to dissolve and precipitate the initial product three times to obtain poly N,N-diethylacrylamide (PDEA).

[0035] 0.005 g of azobisisobutyronitrile, 2.184 g of poly N, N-diethylacrylamide (PDEA) and 1.081 g of acrylamide were weighed and completely dissolved in a 25 mL test tube with 4.4673 g of N, N-dimethylformamide, and then 0.8287 g of N, N-diethylacrylamide (DEA) was added and mixed evenly. After nitrogen with a purity of 99.999% was introduced at room temperature for 15 min, the mixture was sealed and stirred in an oil bath at 70 ° C for 36 h. A mixed solvent of ethyl acetate and n-hexane with a volume ratio of 1:4 was used as a precipitant, and three dissolutions and three precipitations were performed. Subsequently, the mixture was placed in a vacuum oven at 40 ° C until constant weight was obtained, and the temperature-sensitive block [poly N, N-diethylacrylamide-g-poly (N, N-diethylacrylamide-g-acrylamide)] was obtained, which was recorded as PDEA-bP (DEA-co-AM).

[0036] Weigh 0.05 g of the thermosensitive block, 1.12 g of acrylamide, 0.5 g of acrylic acid and 0.1 mmol of template ions (0.0615 mmol of SeO 4 2- , 0.031mmol of In 3+ and 0.0075mmol of Ga 3+) was dissolved in a mixed solvent of water and methanol with a volume ratio of 1:2, and self-assembled for 1 hour in a constant temperature water bath at a temperature of 33°C and a magnetic stirring speed of 150 r / min. 5.5g of N,N-methylenebisacrylamide was added and stirred until completely dissolved. Nitrogen with a purity of 99.999% was introduced at room temperature for 15 minutes and then sealed to form a solution system. The same volume of ammonium persulfate solution with a molar volume concentration of 4.483mmol / L and N,N,N,N-tetramethylethylenediamine solution with a molar volume concentration of 8.964mmol / L were taken and mixed to form an AP-TEMED redox initiator system solution. The redox initiator system AP-TEMED was injected into the solution system with a syringe and then sealed. After initiating polymerization at 35°C, the solution was taken out and placed in a vacuum drying oven to dry to constant weight to obtain the temperature-sensitive multi-template intelligent imprinting polymer GIS-SIIP.

[0037] The dried polymer was crushed by a multifunctional pulverizer, and the particles of 30-100 mesh were sieved with a sieve and stored, and then put into a 200 mesh filter bag (7.6×50 mm), and placed in a Soxhlet extractor to elute the template ions with anhydrous ethanol, and the corresponding template ion concentration in the etching solution was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES) analysis technology. When the test value was lower than 0.02 μg / mL, the elution was stopped, and then the filter bag was alternately rinsed with methanol and water until the solution was neutral, and then placed at 45°C for vacuum drying to constant weight. After drying, adsorbent 3 was obtained.

[0038] The structural characterization and performance evaluation are as follows: Take the temperature-sensitive multi-template intelligent imprinting polymer (GIS-SIIP) prepared in Example 1 as an example.

[0039] Figure 2 The FTIR spectra of PDEA, P(DEA-co-AM) and PDEA-bP(DEA-co-AM) obtained in Example 1 of the present invention are shown. PDEA-bP(DEA-co-AM) can be regarded as two polymers, PDEA and P(DEA-co-AM), connected by chemical bonds to form a long-chain polymer block. However, after synthesizing PDEA, the present application directly synthesizes PDEA-bP(DEA-co-AM) by random copolymerization, and does not involve the separate synthesis of P(DEA-co-AM). From the comparison of the three material spectra, it can be seen that (1) 3415 cm-1 of the random copolymer P(DEA-co-AM) -1 and 3195 cm -1 The stretching vibration characteristic absorption peaks of OH in adsorbed water and NH on AM are at 3415 cm -1 The characteristic peak at 3464cm-1 This is due to the increased water retention capacity of PAM in the block copolymer, the presence of a large number of water molecules, and the weakened association between water molecules and amino groups. (2) 2972cm -1 The methyl group (-CH 3 )The characteristic peak of asymmetric stretching vibration of CH on 2927cm -1 The methylene group (-CH 2 -) Characteristic peak of CH stretching vibration, 2875cm -1 The peak at 1668 cm is the characteristic peak of CH stretching vibration on tertiary carbon. The addition of DEA significantly strengthens the above characteristic peaks, indicating that the content of DEA in the copolymer increases. (3) 1668 cm -1 and 1635 cm -1 The stretching characteristic absorption peaks of the carbonyl group (C=O) on AM and DEA are 1616 cm -1 It is the characteristic peak of the bending vibration of OH in the water molecule and NH on the primary amide. In the random copolymer, the two peaks influence each other, so that the original sharp peak of the carbonyl group in PDEA is covered.

[0040] Figure 3 PDEA-bP(DEA-co-AM) prepared in Example 1 of the present invention 1 H NMR spectrum. According to the structural formula of the polymer and the chemical shift of the characteristic hydrogen of the corresponding monomer, it can be found that 1 H NMR (400 MHz, DMSO- d6) δ7.40 (s, J =80.1 Hz, 0H), 6.99 (s, J = 61.0 Hz, 0H), 3.17 (s, 0H), 1 H NMR (400MHz, DMSO) δ 7.50 (s, 0H), 6.96 (s, J = 80.5 Hz, 1H), 3.17 (s, 1H). All of these are related to the hydrogen of DEA and AM in the polymer, which proves that the synthesized polymer is the target polymer PDEA-bP(DEA-co-AM).

[0041] Figure 4Scanning electron microscope images of the thermosensitive multi-template intelligent imprinted polymer (GIS-SIIP) (left) and the non-imprinted polymer (GIS-NSIIP) (right) prepared in Example 1. As can be seen from the figure, it can be observed that there are many holes on the surface of GIS-SIIP, and the hole distribution is relatively loose. However, there are no obvious holes on the surface of GIS-NSIIP, and the stacking is dense. On the one hand, this morphological difference is due to the change in the interaction between the polymer microparticle interface caused by the self-assembly between the template ions and the functional monomers. At the same time, due to the hydrogen bonding between the functional monomers and the template ions in GIS-SIIP, the hydrogen bonding between the polymer molecular chains is weakened, resulting in a decrease in the interaction between it and the solvent, making phase separation easier, so there are more holes and the surface is looser.

[0042] Figure 5 The adsorption kinetic curves of a) gallium ions, b) indium ions, and c) selenate ions of the thermosensitive multi-template intelligent imprinted polymer adsorbent prepared in Example 1 of the present invention at 25°C, 35°C, and 45°C are shown. The figure shows that GIS-SIIP has a higher adsorption amount at 35°C compared with 25°C and 45°C, which is because the introduction of the thermosensitive block keeps the imprinted pores complete when GIS-SIIP self-assembles at 35°C; when the external temperature changes, the sol / gel phase transition of the thermosensitive block causes the expansion and contraction of the imprinted pores, resulting in a decrease in the adsorption amount.

[0043] Figure 6 The adsorption kinetic curves of a) gallium ions, b) indium ions, and c) selenate ions of the thermosensitive multi-template intelligent imprinted polymer adsorbent prepared in Example 1 of the present invention at 25°C, 35°C, and 45°C are shown. The figure shows that GIS-SIIP has a higher desorption amount at 25°C compared with 35°C and 45°C. This is because when the adsorption temperature T=25°C (lower than the lower critical phase transition temperature of the thermosensitive block), the molecular chain is in a stretched state, so that the imprinted pores are in a relaxed state, the integrity of the imprinted pores deteriorates, the spatial fit between the imprinted pores and the target ions deteriorates, the imprinted sites belong to incomplete imprinted sites, and the affinity of the imprinted pores to the template ions is weakened, so the adsorbed template ions are easily desorbed.

[0044] Take the same volume of selenic acid solution with a molar volume concentration of 0.615mmol / L, 0.31mmol / L indium trichloride solution and 0.075mmol / L gallium trichloride solution and mix them, and use inductively coupled plasma mass spectrometry (ICP-MS) to determine the ion concentration in the solution before adsorption. Take 0.1g of the adsorbent prepared in Example 1 and adsorb it at 35℃ for 120min, then put it into a mixed solution of 0.1mol / L hydrochloric acid (HCl) and 0.3mol / L thiourea (TU), and desorb it at 25℃ for 300min; after repeating the adsorption-desorption cycle 10 times, use inductively coupled plasma mass spectrometry (ICP-MS) to determine the ion concentration after adsorption and the ion concentration after desorption. The results are as follows: Figure 7 As shown in the figure, after 8 adsorption-desorption cycles, the adsorption amount does not change much from the original value, indicating that the temperature-sensitive multi-template intelligent imprinted polymer prepared by the preparation method of the present invention has good reusability.

[0045] 1.00 mL of the flexible copper indium gallium selenide thin film solar cell leachate was diluted 20 times, and then a temperature-sensitive multi-template intelligent imprinting polymer GIS-SIIP was used in the above solution for an adsorption / desorption cycle. The process is as follows: 0.200 g of GIS-SIIP was placed in 20.00 mL of the above flexible copper indium gallium selenide thin film solar cell leachate dilution solution, adsorbed at 35 ° C for 120 min, and then desorbed at 25 ° C for 300 min using a mixed solution of 0.1 mol / L hydrochloric acid (HCl) and 0.3 mol / L thiourea (TU) as a desorbent. The concentration of each element before adsorption and in the desorption solution was determined by inductively coupled plasma mass spectrometry (ICP-MS) and the proportion of each element was calculated. The results are shown in Table 1.

[0046] Table 1 The proportion of each element in the original leaching solution and the proportion of each element in the desorption solution after one adsorption / desorption It can be seen that after one adsorption / desorption cycle, the purity of gallium element increased from 4.38% to 12.77%; the purity of indium element increased from 18.67% to 35.43%; and the purity of selenium element increased from 34.08% to 45.8%, which indicates that GIS-SIIP adsorbent has good separation and purification ability for the target metal elements.

Claims

1. A method for selectively recovering gallium, indium and selenium in proportion from the leachate of flexible copper gallium indium selenide thin film solar cells. It is characterized in that The following steps are involved: 1) PDEA synthesis Azobisisobutyronitrile, 2-(dodecyl trithiocarbonate)-2-methylpropionic acid and N,N-diethylacrylamide are dissolved in ethyl acetate, mixed evenly, and sealed after passing nitrogen for 15-20 minutes. The mixture is stirred in an oil bath at 60-80°C for 30-40 hours. After the reaction is completed, ethyl acetate is used as a solvent and n-hexane is used as a precipitant. The mixture is dissolved and precipitated three times to obtain poly (N,N-diethylacrylamide), which is recorded as PDEA. 2) Synthesis of thermosensitive block of PDEA-bP(DEA-co-AM) Azobisisobutyronitrile, PDEA, acrylamide and N,N-diethylacrylamide were dissolved in N,N-dimethylformamide, mixed evenly, and sealed after nitrogen was passed for 15-20 minutes. The mixture was stirred in an oil bath at 60-80°C for 30-40 hours. Ethyl acetate was used as solvent and n-hexane was used as precipitant. The mixture was dissolved and precipitated three times. The mixture was taken out and placed in a vacuum drying oven to a constant weight, thereby obtaining a thermosensitive block [poly (N,N-diethylacrylamide-g-poly (N,N-diethylacrylamide-g-acrylamide)], which was recorded as PDEA-bP (DEA-co-AM). 3) GIS-SIIP synthesis PDEA-bP (DEA-co-AM), acrylamide, acrylic acid and template ions were dissolved in a mixed solution of methanol and water. After self-assembly in a water bath at 30-35°C for 1-2 hours, a crosslinking agent N,N-methylenebisacrylamide was added, nitrogen was passed through for 15-20 minutes and then sealed. The redox initiation system AP-TEMED was injected into the system with a syringe and then sealed. After initiating polymerization at 30-40°C for 20-25 hours, the system was taken out and placed in a vacuum drying oven to be dried to constant weight to obtain GIS-SIIP. 4) Adsorbent preparation The dried GIS-SIIP was crushed, and the particles of 30-100 mesh were sieved with a sieve and stored, and then put into a 200-mesh filter bag, and placed in a Soxhlet extractor, and the template ions were eluted with analytical pure anhydrous ethanol as the eluent, and the corresponding template ion concentration in the etching solution was determined by ICP-AES. When the test value was lower than 0.02 μg / mL, the elution was stopped, and then the filter bag was alternately rinsed with methanol and water until the solution was neutral, and dried in a vacuum drying oven to constant weight, and the adsorbent was obtained; 5) Ion adsorption / desorption The adsorbent is placed in the leachate of a flexible copper gallium indium selenide thin film solar cell for adsorption, the adsorption temperature is 35°C, and the adsorption time is 120 min; after the adsorption is completed, the adsorbent is placed in a mixed solution containing 0.1 mol / L HCl and 0.3 mol / L thiourea for desorption, the desorption temperature is 25°C, and the desorption time is 300 min; thus, a desorption solution of gallium, indium, and selenium elements recovered in proportion is obtained.

2. A method for selectively recovering gallium, indium and selenium in proportion from a leachate of a flexible copper gallium indium selenide thin film solar cell as claimed in claim 1, It is characterized in that In step 1), the molar ratio of azobisisobutyronitrile, 2-(dodecyltrithiocarbonate)-2-methylpropionic acid and N,N-diethylacrylamide is 1:(15-25):(950-1050).

3. A method for selectively recovering gallium, indium and selenium in proportion from a leachate of a flexible copper gallium indium selenide thin film solar cell as claimed in claim 1, It is characterized in that In step 2), the molar ratio of azobisisobutyronitrile, PDEA and acrylamide is 1:(15-25):(950-1050), and the molar ratio of N,N-diethylacrylamide to acrylamide is 1:1.5-1:2.

5.

4. A method for selectively recovering gallium, indium and selenium in proportion from a leachate of a flexible copper gallium indium selenide thin film solar cell as claimed in claim 1, It is characterized in that In step 3), the mass ratio of PDEA-bP (DEA-co-AM) to acrylic acid is 1:5-1:20, the molar ratio of acrylamide to acrylic acid is 1:2-2:1, and the molar ratio of acrylic acid to N,N-methylenebisacrylamide is 1:5-1:

7.

5. A method for selectively recovering gallium, indium and selenium in proportion from a leachate of a flexible copper gallium indium selenide thin film solar cell as claimed in claim 1, It is characterized in that In step 3), the template ions are a mixed ion system composed of gallium, indium and selenium ions in a molar ratio of 1:4:8, and the amount of template ions added accounts for 30% to 40% of the molar amount of acrylic acid.

6. A method for selectively recovering gallium, indium and selenium in proportion from a leachate of a flexible copper gallium indium selenide thin film solar cell as claimed in claim 1, It is characterized in that In step 3), the AP-TEMED redox initiation system is prepared by mixing equal volumes of an ammonium persulfate solution and an N,N,N,N-tetramethylethylenediamine solution in a molar concentration ratio of 1:

2.

7. A method for selectively recovering gallium, indium and selenium in proportion from a leachate of a flexible copper gallium indium selenide thin film solar cell as claimed in claim 1, It is characterized in that In step 5), the flexible copper gallium indium selenide thin film solar cell leachate refers to a 5 mol / L HCl solution containing 5 vol% hydrogen peroxide as a leachate, which is added to the flexible copper gallium indium selenide thin film solar cell with the outer protective film and substrate removed at a solid-liquid ratio of 5 g / L, and the resultant is leached at 35-45°C for 1-2 hours.

8. A method for selectively recovering gallium, indium and selenium in proportion from a leachate of a flexible copper gallium indium selenide thin film solar cell as claimed in claim 1, It is characterized in that In step 5), proportional recovery means that, except for gallium, indium and selenium, the content of other interfering elements in the analytical solution accounts for less than 10%.

Citation Information

Patent Citations

  • Recovery methods of copper indium gallium selenide

    CN102296178A

  • Method for preparing metal ion imprinting adsorbent with underwater selective recognition performance

    CN102626611A

  • Recovery method of copper indium gallium selenide thin-film solar panel

    CN103184338A

  • Preparation method of molecularly imprinted polymer capable of simultaneously adsorbing multiple nitrides

    CN104877071A

  • Device and method used for measuring selenium in water bodies via molecular imprinting selective laser induced fluorescence

    CN104977282A

Cited By

  • Method for recycling gallium, copper and indium according to proportion in waste thin film photocell and then coating film

    CN121174678A