Preparation method of monodisperse small-particle-size polysiloxane microspheres
By using zwitterionic surfactant and inorganic alkali in the preparation of polysiloxane microspheres for hydrolysis and polycondensation reaction, the problems of complex operation, high equipment corrosion and difficult to control particle size in the prior art are solved, and small particles are realized The efficient preparation of diametric polysiloxane microspheres is characterized by simple operation, environmental protection and low cost.
Patent Information
- Application Number
- CN202411385396.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The existing preparation method for polysiloxane microspheres has the disadvantages of complex operation, high equipment corrosion, high cost, poor environmental pollution and particle size, especially for microspheres with less than 1 μm particle size. .
The zwitterionic surfactant and siloxane monomer were added during hydrolysis, followed by the addition of inorganic alkali solution for polycondensation reaction, and the reaction conditions were controlled to obtain a milky white mixture, and monodispersible small particle size poly The particle size of silicone microspheres can be controlled within the range of 0.6μm-1.3μm.
It realizes the preparation of small-particle-silicon polysiloxane microspheres with simple operation, green and environmentally friendly, low-cost and uniform particle size, avoids the use of acid catalysts, reduces the corrosion of the equipment, and improves the dispersion and uniformity of the particles. .
Smart Images

Figure HDA0005070879390000011 
Figure HDA0005070879390000012 
Figure HDA0005070879390000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of organosilicon microsphere resin, and in particular to a method for preparing monodisperse small-particle-size polysiloxane microspheres. Background Art
[0002] Polysiloxane microspheres are widely used in industrial production such as light diffusers and chemical fillers due to their high hardness and high melting point. With the development of industries such as liquid crystal display, the research and development of polysiloxane microspheres has also attracted more attention. Common methods for preparing polysiloxane microspheres include: one-step sol method, sol-gel method, emulsion polymerization method and addition method. Among them, the one-step sol method and sol-gel method have gained more attention due to their controllable reaction and lower cost. The one-step sol method is that the siloxane monomer directly completes the hydrolysis and polycondensation reaction under the condition of alkaline catalyst, that is, the hydrolysis and polycondensation are carried out simultaneously at the interface of the two phases. The sol-gel method is that the monomer and water are hydrolyzed under certain conditions to form a homogeneous system, and then further polycondensation reaction occurs under the catalysis of alkali to form polymer microspheres with a certain cross-linked structure. The one-step sol method has complex operation, difficulty in maintaining the reaction interface of hydrolysis and polycondensation, and low production efficiency, while the hydrolysis and polycondensation reactions of the sol-gel method are carried out separately, the operation is simpler, and the production efficiency is higher. Therefore, the sol-gel method is more widely used.
[0003] Patent CN1311266A provides a R 1 Si(OR 2 )3 and Si(OR 2 )4 is hydrolyzed under acidic conditions and then an alkaline catalyst solution is added to prepare polysiloxane microspheres. The method can prepare polysiloxane microspheres with an average particle size of 0.1 μm-5 μm, and the experimental results show that the average particle size of the polysiloxane microspheres decreases with the increase of the amount of tetramethoxysilane. The acidic reagent used in this patent is easy to corrode the equipment and has high requirements for the equipment.
[0004] Patent CN1205345A provides a method for preparing polysiloxane microspheres by mixing water, anionic surfactant, polymer stabilizer and hydroxide alkali, adding silane monomer and stirring. The method can prepare polysiloxane microspheres with an average particle size of 0.5μm-10μm, but there are disadvantages such as environmental pollution, increased cost and complicated operation. Patent CN106317409A provides a method for controlling the particle size of polysiloxane microspheres by adjusting the conductivity of deionized water and the molar ratio of deionized water and alkoxysilane. The method can prepare polysiloxane microspheres with an average particle size of 1μm-10μm. Patent CN104744700A provides a method for controlling the particle size of polysiloxane microspheres by adjusting the pH value of the reaction system during the polymerization process. The method can prepare polysiloxane microspheres with an average particle size of 1.5μm-5μm. The above method has certain disadvantages and there is little research on polysiloxane microspheres with an average particle size of less than 1μm. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing polysiloxane microspheres which is simple to operate, environmentally friendly, low in cost and has a small particle size in view of the deficiencies in the prior art.
[0006] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme:
[0007] A method for preparing monodisperse small-size polysiloxane microspheres comprises the following steps:
[0008] (1) Hydrolysis process: Add zwitterionic surfactant to water, stir mechanically to mix evenly, heat to 45°C-65°C in a water bath, add siloxane monomer, stir to react, and obtain silanol solution for standby use;
[0009] (2) Polycondensation process: adding an inorganic alkali solution to the silanol solution obtained in step (1), stirring until the mixed solution turns milky white, and then stopping stirring immediately; placing the milky white liquid in a 40-70° C. water bath for 1-5 hours, and then standing at room temperature for 1-5 hours;
[0010] (3) Drying process: The solid-liquid mixture obtained in step (2) is centrifuged, the lower solid layer is removed, and washed with anhydrous ethanol until neutral. The obtained solid sample is placed in a vacuum drying oven at 100-120° C. and dried for 6 h, and then cooled to room temperature to obtain monodisperse small-particle polysiloxane microspheres.
[0011] The particle size of the monodisperse small-particle polysiloxane microspheres obtained by the invention can be controlled within the range of 0.6 μm to 1.3 μm.
[0012] Preferably, the zwitterionic surfactant in step (1) is a betaine-type zwitterionic surfactant. More preferably, the betaine-type zwitterionic surfactant is selected from at least one of dodecyl hydroxypropyl phosphate betaine, dodecyl dimethyl betaine, tetradecyl sulfonyl betaine, tetradecyl dimethyl betaine, and cocamidopropyl betaine, and further preferably dodecyl dimethyl betaine, tetradecyl sulfonyl betaine, tetradecyl dimethyl betaine, or cocamidopropyl betaine.
[0013] Preferably, the mass ratio of the zwitterionic surfactant to water in step (1) is in the range of 1:18-1:9000, more preferably 1:60-1:1000.
[0014] Preferably, the siloxane monomer in step (1) is methyltrimethoxysilane.
[0015] Preferably, in step (1), the mass ratio of the siloxane monomer to water is in the range of 1:3-1:45, preferably in the range of 1:3-1:15.
[0016] Preferably, the mechanical stirring frequency in step (1) is in the range of 170 rpm-400 rpm, and the stirring time is in the range of 10-50 min.
[0017] Preferably, in step (2), the inorganic base in the inorganic base solution is an alkali metal hydroxide, such as sodium hydroxide, potassium hydroxide, etc., and the solvent is water; the mass concentration of the inorganic base solution is in the range of 0.2%-7%.
[0018] More preferably, the mass ratio of the inorganic base solution in step (2) to the water required for preparing the silanol solution is in the range of 1:2.5-1:70.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] (1) The present invention effectively controls the particle size of the polysiloxane microspheres to be between 0.6 μm and 1.3 μm by regulating the type and addition amount of the zwitterionic surfactant.
[0021] (2) Simple operation and low equipment requirements;
[0022] (3) No acid catalyst is used, which has little corrosion to the equipment;
[0023] (4) No need to add additional polymer stabilizer, which is environmentally friendly;
[0024] (5) The subsequent processing is simple, and the obtained product has a small particle size span, uniform particles and good dispersibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The particle size distribution curve (a) and scanning electron microscope image (b) of the polysiloxane microspheres obtained in Example 1;
[0026] Figure 2 The particle size distribution curve (a) and scanning electron microscope image (b) of the polysiloxane microspheres obtained in Example 2;
[0027] Figure 3 (a) is a particle size distribution curve diagram and (b) a scanning electron microscope diagram of the polysiloxane microspheres obtained in Example 3;
[0028] Figure 4 (a) and a scanning electron microscope image (b) of the particle size distribution curve of the polysiloxane microspheres obtained in Example 4.
[0029] Figure 5 (a) and a scanning electron microscope image (b) of the particle size distribution curve of the polysiloxane microspheres obtained in Example 5.
[0030] Figure 6 (a) and (b) the particle size distribution curve of the polysiloxane microspheres obtained in Comparative Example 1.
[0031] Figure 7 (a) and (b) the particle size distribution curve of the polysiloxane microspheres obtained in Comparative Example 2. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto and may have many variations. If there are any points not particularly described in detail below, they can be understood by those skilled in the art according to conventional expressions or implemented according to existing technologies.
[0033] Example 1
[0034] Add 450g of water and 0.7g of dodecyl hydroxypropyl betaine phosphate to a four-necked flask equipped with a stirring paddle, a thermometer, and a reflux condenser, and heat it to 40°C in a water bath. Add 90g of methyltrimethoxysilane, stir at 200rpm for 10min, add 100mL of 1% sodium hydroxide aqueous solution, continue stirring until the solution turns milky white and stop stirring. The obtained milky white liquid was kept at 55°C for 4h, and centrifuged after standing at room temperature for 3h. Take the lower precipitate, wash it with anhydrous ethanol until it is neutral, and put it in a vacuum drying oven at 120°C for 6h. The average particle size of the obtained polysiloxane microspheres is 1.258μm and the span is 1.04. The reason why the average particle size is greater than 1μm may be related to the spatial position of the dodecyl hydroxypropyl phosphate group in dodecyl hydroxypropyl betaine phosphate.
[0035] Example 2
[0036] Add 450g of water and 2.5g of dodecyl dimethyl betaine to a four-necked flask equipped with a stirring paddle, a thermometer, and a reflux condenser, and heat it in a water bath to 50°C. Add 90g of methyltrimethoxysilane, stir at 170rpm for 10min, then add 120mL of 0.4% sodium hydroxide aqueous solution, continue stirring until the solution turns milky white and stop stirring. The obtained milky white liquid is kept at 55°C for 5h, kept still in 25°C water for 4h, and then centrifuged. Take the lower precipitate and wash it with anhydrous ethanol until it is neutral, and put it in a vacuum drying oven at 120°C and dry it for 6h. The average particle size of the obtained polysiloxane microspheres is 0.683μm and the span is 0.998.
[0037] Example 3
[0038] Add 450g of water and 5g of tetradecyl sulfobetaine to a four-necked flask equipped with a stirring paddle, a thermometer, and a reflux condenser, and heat it in a water bath to 55°C. Add 50g of methyltrimethoxysilane, stir at 250rpm for 10min, then add 150mL of 3% sodium hydroxide aqueous solution, continue stirring until the solution turns milky white and stop stirring. Keep the obtained milky white liquid at 55°C for 4h, keep it at room temperature for 5h, and then centrifuge it. Take the lower precipitate, wash it with anhydrous ethanol until it is neutral, and put it in a vacuum drying oven at 100°C for 6h. The average particle size of the obtained polysiloxane microspheres is 0.711μm and the span is 0.911.
[0039] Example 4
[0040] Add 450g of water and 7g of tetradecanedimethyl betaine to a four-necked flask equipped with a stirring paddle, a thermometer, and a reflux condenser, and heat it in a water bath to 40°C. Add 100g of methyltrimethoxysilane, stir at 400rpm for 10min, then add 120mL of 5% sodium hydroxide aqueous solution, continue stirring until the solution turns milky white and stop stirring. Keep the obtained milky white liquid at 60°C for 5h, keep it at room temperature for 3h, and then centrifuge it. Take the lower precipitate, wash it with anhydrous ethanol until it is neutral, and dry it in a vacuum drying oven at 120°C for 6h. The average particle size of the obtained polysiloxane microspheres is 0.743μm and the span is 1.283.
[0041] Example 5
[0042] Add 450g of water and 0.5g of cocamidopropyl betaine to a four-necked flask equipped with a stirring paddle, a thermometer, and a reflux condenser, and heat it in a water bath to 55°C. Add 50g of methyltrimethoxysilane, stir at 300rpm for 30min, then add 8mL of 0.5% sodium hydroxide aqueous solution, continue stirring until the solution turns milky white and stop stirring. Keep the obtained milky white liquid at 55°C for 5h, keep it at room temperature for 3h, and then centrifuge it. Take the lower precipitate, wash it with anhydrous ethanol until it is neutral, and put it in a vacuum drying oven at 120°C for 6h. The average particle size of the obtained polysiloxane microspheres is 0.634μm and the span is 1.082.
[0043] Comparative Example 1: Preparation of polysiloxane microspheres using nonionic surfactants
[0044] Add 450g of water and 0.5g of alkylphenol polyoxyethylene ether to a four-necked flask equipped with a stirring paddle, a thermometer, and a reflux condenser, and place it in a water bath and heat it to 55°C. Add 50g of methyltrimethoxysilane, stir at 300rpm for 30min, then add 8mL of 5% sodium hydroxide aqueous solution, continue stirring until the solution turns milky white and stop stirring. Keep the obtained milky white liquid at 55°C for 5h, keep it at room temperature for 3h, and then centrifuge it. Take the lower precipitate, wash it with anhydrous ethanol until it is neutral, and put it in a vacuum drying oven at 120°C for 6h. The average particle size of the obtained polysiloxane microspheres is 2.823μm and the span is 1.433.
[0045] Comparative Example 2: Preparation of polysiloxane microspheres using phenyltrimethoxysilane
[0046] Add 450g of water and 2.5g of dodecyl dimethyl betaine to a four-necked flask equipped with a stirring paddle, a thermometer, and a reflux condenser, and heat it to 50°C in a water bath. Add 50g of phenyltrimethoxysilane, stir at 170rpm for 10min, then add 120mL of 0.4% sodium hydroxide aqueous solution, continue stirring until the solution turns milky white and stop stirring. The obtained milky white liquid was kept warm at 55°C for 5h, kept warm in 25°C water for 4h, and then centrifuged. Remove the lower precipitate and wash it with anhydrous ethanol until it is neutral, and place it in a vacuum drying oven at 120°C and dry it for 6h. The obtained polysiloxane microspheres are severely agglomerated, and the accurate average particle size and span cannot be measured.
Claims
1. A method for preparing monodisperse small-size polysiloxane microspheres, characterized in that: The preparation method comprises the following steps: (1) Hydrolysis process: Add zwitterionic surfactant to water, stir mechanically to mix evenly, heat to 45°C-65°C in a water bath, add siloxane monomer, stir to react, and obtain silanol solution for standby use; (2) Polycondensation process: adding an inorganic alkali solution to the silanol solution obtained in step (1), stirring until the mixed solution turns milky white, and then stopping stirring immediately; placing the milky white liquid in a 40-70° C. water bath for 1-5 hours, and then standing at room temperature for 1-5 hours; (3) Drying process: The solid-liquid mixture obtained in step (2) is centrifuged, the lower solid layer is removed, and washed with anhydrous ethanol until neutral. The obtained solid sample is placed in a vacuum drying oven at 100-120° C. and dried for 6 h, and then cooled to room temperature to obtain monodisperse small-particle polysiloxane microspheres.
2. The preparation method according to claim 1, characterized in that: The particle size of the monodisperse small-particle polysiloxane microspheres is in the range of 0.6 μm to 1.3 μm.
3. The preparation method according to claim 1 or 2, characterized in that: The zwitterionic surfactant in step (1) is a betaine type zwitterionic surfactant.
4. The preparation method according to claim 3, characterized in that: The betaine type zwitterionic surfactant is selected from at least one of dodecyl hydroxypropyl phosphate betaine, dodecyl dimethyl betaine, tetradecyl sulfobetaine, tetradecanedimethyl betaine and cocamidopropyl betaine.
5. The preparation method according to claim 4, characterized in that: The betaine type zwitterionic surfactant is selected from dodecyl dimethyl betaine, tetradecyl sulfobetaine, tetradecanedimethyl betaine or cocamidopropyl betaine.
6. The preparation method according to claim 1 or 2, characterized in that: The mass ratio of the zwitterionic surfactant to water in step (1) is in the range of 1:18-1:9000, preferably 1:60-1:1000.
7. The preparation method according to claim 1 or 2, characterized in that: The siloxane monomer in step (1) is methyltrimethoxysilane.
8. The preparation method according to claim 1 or 2, characterized in that: In step (1), the mass ratio of siloxane monomer to water is in the range of 1:3-1:
45.
9. The preparation method according to claim 1 or 2, characterized in that: In step (2), in the inorganic alkali solution, the inorganic alkali is an alkali metal hydroxide and the solvent is water; the mass concentration of the inorganic alkali solution is in the range of 0.2%-7%.
10. The preparation method according to claim 9, characterized in that: The mass ratio of the inorganic alkali solution in step (2) to the water required for preparing the silanol solution is in the range of 1:2.5-1:70.
Citation Information
Patent Citations
Preparation method of mono-dispersion polysiloxane microspheres with controllable particle size
CN104744700A
Preparing method of polyorganosiloxane microsphere
CN106317409A
Process for preparing polysiloxane microspheres with narrow size distribution
CN1205345A
Ball shaped granular of polyorganosiloxane, and its prepn. method
CN1311266A
Method for preparing narrow-size-dispersion ultrafine polyvinyl siloxane crosslinked microspheres
CN106432733A