Selective lead stabilizing agent of thiosemicarbazide modified chitosan embedded sodium alginate as well as preparation method and application of selective lead stabilizing agent

By modifying chitosan-embedded sodium alginate selective lead stabilizer in thiourea-modified chitosan, the problems of insufficient adsorption capacity of heavy metal stabilizers in the prior art and great impact on soil are solved, and efficient and selective adsorption are achieved. The effect of lead reduces the risk of heavy metal oozing and simplifies the preparation process.

CN119039624APending Publication Date: 2024-11-29ZHEJIANG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411378861.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing heavy metal stabilizers have weak adsorption capacity in soil repair, require high dosage, and have a negative impact on soil structure and fertility. They lack selectivity for specific heavy metals, making it difficult to effectively control the risk of heavy metal leaching.

Method used

Develop a selective lead stabilizer with thiourea-modified chitosan embedded sodium alginate through specific preparation methods to embed sodium alginate in thiourea-modified chitosan to form efficient lead adsorption compounds used to stabilize heavy metals in soil.

Benefits of technology

It achieves efficient and selective adsorption and stabilization of lead in the soil, reduces the risk of heavy metal leaching, does not affect phytorepair and the extraction of other heavy metals, simplifies the preparation process, and reduces the impact on the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039624A_ABST
    Figure CN119039624A_ABST
Patent Text Reader

Abstract

The invention discloses a selective lead stabilizing agent of thiosemicarbazide modified chitosan embedded sodium alginate as well as a preparation method and application of the selective lead stabilizing agent. The preparation method comprises the following steps: cross-linking chitosan and thiosemicarbazide under the action of glutaraldehyde to generate thiosemicarbazide modified chitosan (TC-CS), cross-linking sodium alginate and TC-CS powder with a mixed solution in the presence of EDC and NHS through calcium chloride to form composite microspheres (TC-CS / SA), washing the calcium chloride with deionized water, and carrying out cold drying to obtain a final product. The preparation method is simple, and reaction conditions are mild; the used raw materials chitosan and sodium alginate are green and easy to obtain; the obtained stabilizing agent can efficiently, rapidly and selectively adsorb Pb, can effectively stabilize Pb in soil, reduces toxicity to plants, and cooperates with the plants to repair Pb in sludge.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of heavy metal stabilizers in heavy metal pollution treatment of soil, and in particular to a selective lead stabilizer of thiosemicarbazide-modified chitosan-embedded sodium alginate, and a preparation method and application thereof. Background Art

[0002] Municipal sewage sludge is one of the main by-products of municipal sewage treatment plants. Due to the pathogens, heavy metals and other pollutants contained in the sludge, its land use is restricted. In particular, heavy metal elements (such as zinc, copper, lead, nickel, and cadmium) pose a serious threat to the environment and human health. These heavy metal ions can enter the soil through leaching after rainfall, resulting in an increase in the heavy metal content of the soil, among which the content of lead (Pb) is particularly prominent. At present, although there are a variety of heavy metal removal methods such as chemical, biological and physical methods, these methods are generally not efficient in removing heavy metal ions in sludge, and a large amount of heavy metal ions still remain in the treated sludge. Therefore, heavy metal stabilization has become one of the most effective and direct methods to control the risk of heavy metal leaching.

[0003] Existing heavy metal solidifiers, including lime, phosphate, zeolite and montmorillonite, have been widely used in the field of soil remediation. These solidifiers interact with heavy metal ions through chemical and physical mechanisms, reducing their solubility and bioavailability. However, their adsorption capacity is relatively weak, resulting in the need for higher dosages, which increases treatment costs and has a negative impact on soil structure and fertility. For example, the use of lime may lead to an increase in soil pH, affecting soil microbial activity and plant growth. Excessive use of phosphates may lead to an excess of phosphorus in the soil, affecting plant nutrient absorption and water quality. Although zeolite and montmorillonite can effectively adsorb heavy metal ions, their adsorption capacity is affected by soil pH and ionic strength, which may change the porosity and water vapor retention capacity of the soil.

[0004] In contrast, biochar, a carbon-based material obtained by thermal cracking of biomass, shows great potential in the remediation of soil heavy metal pollution due to its high specific surface area and chemical stability. Biochar can effectively adsorb and fix heavy metal ions, reducing their migration and bioavailability in the environment. However, the use of biochar also faces challenges. First, the preparation process of biochar requires precise control of conditions, which increases the complexity of production. Second, the adsorption effect of biochar on different heavy metals may vary, and it needs to be optimized and selected for specific pollution situations. In addition, the production and use of biochar may generate carbon emissions, which need to be reduced by using renewable energy and optimizing the production process.

[0005] In summary, although existing curing agents have played a certain role in the remediation of heavy metal contaminated soil, their high dosage, potential negative impact on soil, and lack of selectivity for heavy metals limit their widespread use in practical applications. Therefore, the development of new curing agents with higher adsorption capacity and selectivity for specific heavy metals, while reducing the impact on the environment, is an urgent problem to be solved in the current and future soil remediation field. Chitosan is a natural polysaccharide formed by deacetylation of chitin. The amino (-NH2) and hydroxyl (-OH) functional groups in its molecular chain provide abundant adsorption active sites, which makes chitosan have significant adsorption properties for heavy metal ions. Sodium alginate (SA) is a natural polysaccharide derived from brown algae, known for its excellent biocompatibility, biodegradability and renewability. The hydroxyl and carboxyl functional groups in the molecular structure of sodium alginate give it a strong adsorption affinity for heavy metal ions. Combining the properties of chitosan and sodium alginate, developing a chitosan-encapsulated sodium alginate biostabilizer can provide a new and selective method for stabilizing lead (Pb) in soil, providing an innovative solution in the field of soil heavy metal remediation. Summary of the invention

[0006] The present invention aims to overcome at least one of the shortcomings and deficiencies of the above-mentioned prior art, and provides a selective lead stabilizer of sodium alginate embedded in chitosan modified by thiosemicarbazide, and a preparation method and application thereof, wherein the prepared compound can selectively adsorb and effectively stabilize Pb in soil. The purpose of the present invention is achieved based on the following technical solutions:

[0007] The first aspect of the present invention provides a method for preparing a semicarbazide-modified chitosan-embedded sodium alginate selective heavy metal stabilizer.

[0008] Preferably, the preparation method specifically comprises the following steps:

[0009] S1: Disperse chitosan powder evenly in acetic acid aqueous solution, and then continue stirring at a temperature range of 20°C to 40°C until the chitosan is completely dissolved;

[0010] S2: extracting the mixed solution obtained in step S1 with a syringe and adding it dropwise to the pre-prepared sodium hydroxide aqueous solution, thereby preparing chitosan microspheres. Subsequently, the formed microspheres are allowed to stand at room temperature to promote further stabilization;

[0011] S3: washing the microspheres obtained in step S2 with ultrapure water until they are neutral, then adding glutaraldehyde aqueous solution and introducing thiosemicarbazide thereto, stirring at a constant temperature of 20° C. to 40° C. for 24 to 48 hours, and obtaining a white powdery substance through post-treatment A;

[0012] S4: Sodium alginate, EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride), and NHS (N-hydroxysuccinimide) are mixed in ultrapure water and stirred at a temperature range of 20°C to 40°C for 1 to 3 hours. Then, the white powder obtained in step S3 is added to the mixture.

[0013] Continue stirring for 10 to 18 hours;

[0014] S5: extracting the mixed solution in step S4 with a syringe and adding it dropwise to the calcium chloride aqueous solution to form composite microspheres, and allowing the formed microspheres to stand to enhance their stability;

[0015] S6: The microspheres formed in step S5 are transferred to a beaker and washed with ultrapure water to remove the residues. Subsequently, the microspheres are placed in a mixed solution of glutaraldehyde and hydrochloric acid and stirred for 24 to 48 hours, and the final product is prepared through post-treatment B.

[0016] Preferably, the volume percentage concentration of the acetic acid aqueous solution in step S1 is preferably between 2% and 5%, and the ratio of the chitosan powder to the acetic acid aqueous solution is preferably 1.0 g of chitosan powder to 30 mL to 60 mL of the acetic acid aqueous solution.

[0017] Preferably, the concentration of the sodium hydroxide aqueous solution in step S2 is in the range of 0.3 mol / L to 0.8 mol / L, and the standing time lasts for 16 to 20 hours.

[0018] Preferably, the volume percentage concentration of the glutaraldehyde aqueous solution in step S3 is preferably between 2.0% and 5%, and the ratio of the glutaraldehyde aqueous solution to thiosemicarbazide is preferably 300mL to 320mL of glutaraldehyde aqueous solution to 1.0g of thiosemicarbazide. In addition, the post-treatment A includes washing the microspheres three times with 300mL to 500ml of ultrapure water, and then placing the washed microspheres in a vacuum oven, drying them at 50°C to 80°C for 24 hours to 48 hours, and then grinding them into powder.

[0019] Preferably, the mass ratio of sodium alginate, EDC, NHS, ultrapure water and white powder in step S4 is (0.01 to 0.02): (0.002 to 0.010): (0.002 to 0.005): 1.0: (0.005 to 0.008).

[0020] Preferably, in step S5, the concentration of the calcium chloride aqueous solution ranges from 0.05 mol / L to 0.15 mol / L, and the standing time is from 16 hours to 20 hours.

[0021] Preferably, in step S6, the volume percentage concentration of glutaraldehyde in the mixed solution is 2.0% to 4.0%, the concentration of hydrochloric acid is 0.05 mol / L to 0.15 mol / L, and the post-treatment B includes washing the microspheres three times with 300 mL to 500 ml of ultrapure water until neutral, and placing them in a cold dryer for cold drying.

[0022] The second aspect of the present invention provides a semicarbazide-modified chitosan-embedded sodium alginate selective heavy metal stabilizer, which is prepared according to the above preparation method.

[0023] The third aspect of the present invention provides an application of a semicarbazide-modified chitosan-embedded sodium alginate selective heavy metal stabilizer in combination with ryegrass to repair Pb in sludge and control the risk of heavy metal Pb leaching in sludge.

[0024] An application of a selective heavy metal stabilizer in the treatment of soil heavy metal pollution, the application method comprising:

[0025] a) applying the stabilizer according to claim 8 uniformly to the soil contaminated by heavy metals at a dosage of 0.5‰ to 2.0‰;

[0026] b) Thoroughly mix the stabilizer with the soil by appropriate soil handling techniques, such as stirring or mixing, to ensure uniform dispersion of the stabilizer;

[0027] c) using the mixed soil to grow plants under suitable conditions, such as suitable temperature and humidity, to evaluate the effects of the stabilizer on soil quality and plant growth;

[0028] d) Monitoring of heavy metal levels in soil and plant tissues to assess stabilization effectiveness.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention uses chitosan, sodium alginate and thiosemicarbazide as raw materials, firstly generates thiosemicarbazide-modified chitosan by cross-linking chitosan and thiosemicarbazide with glutaraldehyde, then embeds sodium alginate in thiosemicarbazide-modified chitosan by amide reaction and cross-linking of calcium ions, and finally washes with ultrapure water and freeze-dries to obtain the final product. Compared with the existing metal stabilizer, the heavy metal selective stabilizer prepared by the present invention has a simple synthesis process and mild reaction conditions, can efficiently, quickly and selectively adsorb Pb, effectively control the leaching risk of heavy metal Pb in sludge compost soil, and does not affect the phytoremediation extraction of other heavy metals in the soil. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a SEM image of the product prepared in Example 1 of the present invention.

[0032] Figure 2 This is the SEM image of the product prepared in Example 2 of the present invention.

[0033] Figure 3 This is the SEM image of the product prepared in Example 3 of the present invention.

[0034] Figure 4 This is the EDS spectrum of the product prepared in Example 1 of the present invention.

[0035] Figure 5 is the chemical reaction formula of the product prepared in Example 1 of the present invention.

[0036] Figure 6 This is the BET diagram of the product prepared in Example 1 of the present invention.

[0037] Figure 7 This is the XRD pattern of the product prepared in Example 1 of the present invention.

[0038] Figure 8 It is the FTIR spectrum of the stabilizer of the present invention.

[0039] Fig. 9 The stabilizer of the present invention has an effect on Pb under different pH conditions. 2+ The adsorption condition.

[0040] Fig.10 The mixed metal selectivity comparison of the stabilizer of the present invention is shown in FIG.

[0041] Fig.11 The stabilizer of the present invention is 2+ The adsorption equilibrium curve.

[0042] Fig.12 The stabilizer of the present invention is 2+ The adsorption kinetics curve. DETAILED DESCRIPTION

[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Example 1

[0045] The chitosan powder of 0.5g is added to the acetic acid aqueous solution of 2% by volume concentration of 25ml, and magnetic stirring is carried out for 2 hours at 25 ℃. After dissolving completely, the mixed solution is extracted with a 10ml syringe, and dripped into the sodium hydroxide aqueous solution of 0.5mol / L to form chitosan microspheres, which are placed for 16 hours to make it more stable. The chitosan microspheres are washed with ultrapure water to neutrality, added to the glutaraldehyde aqueous solution of 2.5% by volume concentration of 100ml, and then 0.320g of thiosemicarbazide is added thereto, and stirred for 24 hours at 25 ℃. The bead is taken out and put into a beaker, washed three times with the ultrapure water of 400ml, put into a vacuum oven and dried, dried at 60 ℃ for 24 hours, and after drying completely, ground to powder (named as TC-CS-1).

[0046] Weigh 0.3g of sodium alginate and add it to 20ml of ultrapure water, add 0.1g of EDC and 0.08g of NHS, stir magnetically for 1 hour at 25°C, then add 0.15g of TC-CS-1 powder and stir for 12 hours. Use a 10ml syringe to extract the mixed solution, drop it into a 0.1mol / L calcium chloride aqueous solution to form composite microspheres, and place it for 12 hours to make it more stable. Put the microspheres in a beaker, wash them three times with 400ml of ultrapure water to wash away the calcium chloride, and then put them into a mixed solution of 100ml of 2.5% glutaraldehyde and 0.1mol / L HCl by volume, and stir for 24 hours. Put the microspheres in a beaker, wash them three times with 400ml of ultrapure water until neutral, put them in an ultra-low temperature refrigerator and freeze them for 2 hours, then take them out, and put them in a cold dryer to dry them for 48 hours until they are completely dried to obtain the final product (TC-CS / SA-1).

[0047] Example 2

[0048] The chitosan powder of 0.7g is added to 45ml 2.5% acetic acid aqueous solution, under 30 ℃, magnetic agitation is 3 hours, after dissolving completely, extracts mixed solution with 10ml syringe, drips into 0.6mol / L sodium hydroxide aqueous solution, forms chitosan microsphere, places 18 hours, makes it more stable.The chitosan microsphere is washed to neutrality with ultrapure water, joins 130ml 3.0% glutaraldehyde aqueous solution, then adds 0.448g thiosemicarbazide wherein, stirs 36 hours under 30 ℃.Bead is taken out and put into beaker, washs three times with the ultrapure water of 400ml, puts into vacuum oven and is dried, dried 3 hours under 80 ℃, after drying completely, is ground to powder (named as TC-CS-2).

[0049] Weigh 0.3g of sodium alginate and add it to 20ml of ultrapure water, add 0.1g of EDC and 0.08g of NHS, stir magnetically for 1 hour at 25°C, then add 0.15g of TC-CS-2 powder and stir for 12 hours. Extract the mixed solution with a 10ml syringe, drop it into a 0.1mol / L calcium chloride aqueous solution to form composite microspheres, and place it for 18 hours to make it more stable. Put the microspheres into a beaker, wash them three times with 400ml of ultrapure water to wash away the calcium chloride, and then put them into a mixed solution of 100ml of 2.5% glutaraldehyde and 0.1mol / LHCl and stir for 36 hours. Put the microspheres into a beaker, wash them three times with 400ml of ultrapure water until neutral, put them into an ultra-low temperature refrigerator and freeze them for 3 hours before taking them out, and then put them into a cold dryer and freeze them for 48 hours until they are completely dried to obtain the final product (TC-CS / SA-2).

[0050] Example 3

[0051] The chitosan powder of 0.5g is added to 25ml of 2% acetic acid aqueous solution, under 25 ℃, magnetic stirring is 2 hours, after dissolving completely, extracts mixed solution with 10ml syringe, drips into 0.5mol / L sodium hydroxide aqueous solution, forms chitosan microsphere, places 20 hours, makes it more stable.The chitosan microsphere is washed to neutrality with ultrapure water, joins 100ml of 2.5% glutaraldehyde aqueous solution, then adds 0.320g of thiosemicarbazide wherein, stirs 48 hours under 25 ℃.The bead is taken out and put into beaker, washs three times with 400ml of ultrapure water, puts into vacuum oven and is dried at 60 ℃ for 48 hours, after drying completely, is ground to powder (named as TC-CS-3).

[0052] Weigh 0.4g of sodium alginate and add it to 30ml of ultrapure water, add 0.15g of EDC and 0.10g of NHS, stir magnetically for 2 hours at 30°C, then add 0.20g of TC-CS-3 powder and stir for 16 hours. Extract the mixed solution with a 10ml syringe and drop it into a 0.15mol / L calcium chloride aqueous solution to form composite microspheres, which are placed for 36 hours to make them more stable. Put the microspheres in a beaker, wash them three times with 400ml of ultrapure water to wash away the calcium chloride, and then put them in a mixed solution of 150ml of 2.5% glutaraldehyde and 0.1mol / L HCl and stir for 36 hours. Put the microspheres in a beaker, wash them three times with 400ml of ultrapure water until neutral, put them in an ultra-low temperature refrigerator and freeze them for 4 hours before taking them out, and then put them in a cold dryer and freeze them for 48 hours until they are completely dried to obtain the final product (TC-CS / SA-3).

[0053] Example 4

[0054] Weigh 0.1599g of lead nitrate, add ultrapure water, dissolve completely in an ultrasonic machine, transfer to a 1000ml volumetric flask, rinse three times with ultrapure water in the wash bottle, and finally adjust the volume to prepare 100mg / L Pb 2+ Solution.

[0055] The pH was adjusted with 0.1 mol / L nitric acid aqueous solution and 0.1 mol / L sodium hydroxide aqueous solution. A total of six pH values ​​were set, namely 2.5, 3.5, 4.5, 5.5, 6.0, and 6.5. Three sets of parallel samples were set for each pH value. 25 ml of heavy metal solution was placed in a conical flask, and then 15 mg of material was added and immediately moved to a constant temperature shaker (25 ° C, 150 rpm) for 2 hours. The supernatant was filtered through a 0.45 μm filter membrane, and the supernatant after the membrane was diluted a certain multiple to determine Pb 2+ Concentration. Based on the measured Pb 2+ The concentration of TC-CS / SA-1 was plotted against Pb at different pH conditions. 2+ The adsorption condition.

[0056] Example 5

[0057] Weigh 0.3802g, 0.4550g, 0.1599g, 0.4955g and 0.2744g of copper nitrate trihydrate, zinc nitrate hexahydrate, lead nitrate, nickel nitrate hexahydrate and cadmium nitrate tetrahydrate, add ultrapure water together, completely dissolve in an ultrasonic machine, transfer to a 1000ml volumetric flask, rinse three times with ultrapure water in a wash bottle, and finally make up to volume to prepare a 100mg / L mixed metal solution. Similarly, prepare 50mg / L, 150mg / L and 200mg / L mixed heavy metal solutions.

[0058] The pH of all mixed solutions was adjusted to 6.0, and three parallel samples were set for each concentration. 25 ml of heavy metal solution was placed in a conical flask, and then 15 mg of TC-CS / SA-1 was added and immediately moved to a constant temperature shaker (25°C, 150 rpm) for 2 hours. The supernatant was filtered through a 0.45 μm filter membrane, and the supernatant after the membrane was diluted a certain multiple and then the Pb 2+ Concentration. Calculate the Pb concentration at different concentrations. 2+ Adsorption amount. According to Pb 2+ Concentration and corresponding Pb 2+ The adsorption equilibrium curve was drawn based on the adsorption amount.

[0059] 0.015 g of TC-CS / SA-1 prepared in Example 1 was added to 25 mL of 100 mg / L lead nitrate aqueous solution and shaken at 25 °C for 2.5 h. During this period, an appropriate amount of the supernatant was filtered through a 0.45 μm filter membrane at intervals of 1, 2, 5, 10, 20, 50, 70, 90, 120, and 150 minutes, and the supernatant after the membrane was diluted a certain multiple before determining the Pb 2+ Concentration. Based on the measured Pb 2+ The adsorption kinetics curve was drawn based on the concentration.

[0060] Example 6

[0061] A total of three groups were set up for the potted experiment, with three parallel samples in each group. 1 kg of soil was added to each pot, of which no material was added to the control group CK, and 0.5‰ (weight ratio) and 2‰ of TC-CS / SA-1 were added to the other two groups, respectively, and mixed thoroughly with the soil. Spread a layer of absorbent paper on the culture dish, add an appropriate amount of tap water, and then spread the ryegrass seeds on the paper. After about 7 days, the seeds germinated into seedlings. In each pot, 25 seedlings with similar growth conditions were transplanted. During the growth period of ryegrass, the same amount of water was poured every day or every other day depending on the soil moisture conditions. A total of 80 days from transplantation to harvesting.

[0062] After the plants were harvested, they were rinsed with deionized water and their plant heights were measured. The results are shown in Table 1.

[0063] The samples were placed in an oven and dried at 105°C for 30 minutes, then the temperature was adjusted to 60°C for further drying for 24 hours. After the plant samples were digested and acid driven, the Pb content in the plants was determined. The results are shown in Table 1.

[0064] Table 1 Average biomass of ryegrass and Pb concentration in plants

[0065]

[0066] From the experimental results, it can be seen that the stabilizer in the present invention not only promotes the growth of ryegrass, but also reduces the concentration of Pd in ​​ryegrass, which shows that the stabilizer successfully stabilizes Pb in the soil and reduces its toxic effect on plants.

[0067] like Figure 1-Figure 3 As shown in the figure, TC-CS / SA shows a layered stacking state under a scanning electron microscope (SEM), which suggests that the original internal morphology of the material should be a layered network structure. When the layered structure is magnified to 1μm, it can be found that it is full of holes, which are uniform in size, densely distributed, and have a diameter of about 20 to 25nm.

[0068] like Figure 4As shown, the element proportion analysis of TC-CS / SA-1 was performed by energy dispersive spectrometer (EDS) to obtain the content and atomic number ratio of carbon, nitrogen, sulfur, hydrogen, oxygen and other elements in the material, as shown in Table 2. The weight proportion of S is 1.41%, indicating that thiosemicarbazide is successfully grafted onto chitosan.

[0069] Table 2 Elemental analysis of TC-CS / SA-1

[0070]

[0071] like Figure 5 As shown in the figure, chitosan, methylthiourea and glutaraldehyde were used as raw materials to modify chitosan through polymerization reaction, and then sodium alginate was embedded and cross-linked with CaCl2 to prepare heavy metal stabilizer microspheres. According to the chemical reaction formula, the chemical structure of the product is inferred to be C 97 H 134 Ca4N4Na4O 67 S. The C:N:O:S=97:4:67:1 in the structural formula is highly consistent with the element ratios of carbon, nitrogen, oxygen, and sulfur recorded in Table 2, which indicates that the synthesized material is consistent with the experimental design and verifies the effectiveness of the preparation process.

[0072] like Figure 6 As shown in Figure 2, the specific surface area and pore volume of TC-CS / SA-1 are 10.34 m 2 / g and 0.069cm 3 / g. The average pore size of TC-CS / SA-1 was determined to be 26.86nm, proving that TC-CS / SA material is a mesoporous adsorbent.

[0073] like Figure 7 As shown, TC-CS / SA-1 has two diffraction peaks at 13.6° and 20.8°, but both are large peaks with serious broadening phenomenon and no fine spectral peak structure, indicating that the crystallinity of TC-CS / SA is very low and it is an amorphous material.

[0074] like Figure 8 As shown, 3318cm in SA -1 The peak at 3367 cm-1 was shifted to 3367 cm-1 in TC-CS / SA-1. -1 This indicates that -NH2 was successfully introduced into the composite of SA and TC-CS. -1 The peak corresponding to -COO- shifted to 1725cm -1 At 1635cm -1 A new peak is generated at 1402 cm, which is caused by the stretching vibration of -C=N in TC-CS. -1 The peak near the-1 , and at 1237cm -1 The characteristic peak of thiourea group in TC-CS was observed at 1725 cm -1 Asymmetric -COO- and 1635cm -1 The doublet of -C=N at 1570 cm-1 was transformed into a singlet and shifted to 1570 cm-1. -1 After Pb adsorption, 1370cm -1 The absorption peaks of the symmetrical -COO- group at 1237 cm -1 The characteristic peaks of thiourea group at -1 and 1321cm -1 This indicates that -COO, C=N and thiourea groups are involved in the adsorption process of Pb.

[0075] like Fig. 9 As shown, TC-CS / SA exhibits a strong adsorption capacity for Pb, and at pH = 6.5, the maximum adsorption amount reaches 151 mg / g.

[0076] like Fig.10 As shown in the figure, the adsorption of Pb by TC-CS / SA is much higher than that of other heavy metals. The order of the adsorption of five heavy metals by TC-CS / SA is as follows: Pb>Cu>Zn>Cd>Ni. As the concentration of each metal in the solution increases, the adsorption of Pb gradually increases, while the adsorption of the other four metals gradually decreases.

[0077] like Fig.11 As shown in Figure 2, TC-CS / SA increases with the initial Pb 2+ With the increase of solution concentration, the adsorption amount gradually increased, and finally the maximum adsorption amount of TC-CS / SA reached 263.9 mg / g.

[0078] like Fig.12 As shown in Figure 2, TC-CS / SA has an effect on Pb 2+ All of them have a fast adsorption speed, and can basically reach adsorption equilibrium in 70 minutes. The good adsorption rate and adsorption capacity indicate that the prepared materials are effective in adsorbing and stabilizing Pb in environmental pollution. 2+ It has good application prospects.

Claims

1. A method for preparing a selective lead stabilizer of thiosemicarbazide-modified chitosan-embedded sodium alginate, characterized in that: The following steps are involved: S1: evenly dispersing chitosan powder in an acetic acid aqueous solution, and then continuously stirring at a temperature range of 20° C. to 40° C. until the chitosan is completely dissolved to obtain a mixed solution; S2: adding the mixed solution obtained in step S1 dropwise into a pre-prepared sodium hydroxide aqueous solution to prepare chitosan microspheres, and then letting it stand to obtain microspheres after stabilization; S3: washing the microspheres obtained in step S2 until they are neutral, then adding a glutaraldehyde aqueous solution and introducing thiosemicarbazide, stirring at a constant temperature of 20° C. to 40° C. for 24 to 48 hours, and obtaining a white powder through post-treatment A; S4: Sodium alginate, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and N-hydroxysuccinimide are mixed in water, and stirred at a temperature range of 20° C. to 40° C. for 1 to 3 hours, and then the white powder obtained in step S3 is added, and stirring is continued for 10 to 18 hours to obtain a reaction mixture; S5: adding the reaction mixture in step S4 dropwise to a calcium chloride aqueous solution to form composite microspheres, and then allowing to stand to form microspheres; S6: The microspheres formed in step S5 are transferred to a reactor, washed, and then placed in a mixed solution of glutaraldehyde and hydrochloric acid and stirred for 24 to 48 hours, and a selective lead stabilizer of aminothiourea-modified chitosan-embedded sodium alginate is obtained through post-treatment B.

2. The preparation method according to claim 1, characterized in that: In step S1, the volume percentage concentration of the acetic acid aqueous solution is 2% to 5%; The dosage ratio of the chitosan powder to the acetic acid aqueous solution is 1.0 g: 30 mL to 60 mL.

3. The preparation method according to claim 1, characterized in that: In step S2, the concentration of the sodium hydroxide aqueous solution ranges from 0.3 mol / L to 0.8 mol / L; The standing time is 16 to 20 hours.

4. The preparation method according to claim 1, characterized in that: In step S3, the volume percentage concentration of the glutaraldehyde aqueous solution is 2.0% to 5%; The ratio of the glutaraldehyde aqueous solution to thiosemicarbazide is 300 mL to 320 mL: 1.0 g; The post-treatment A comprises: washing with ultrapure water, then placing the washed microspheres in a vacuum oven, drying at 50° C. to 80° C. for 24 to 48 hours, and then grinding into powder to obtain white powder.

5. The preparation method according to claim 1, characterized in that: In step S4, the mass ratio of the sodium alginate, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, water and white powder is 0.01-0.02: 0.002-0.010: 0.002-0.005: 1.0: 0.005-0.

008.

6. The preparation method according to claim 1, characterized in that: In step S5, the concentration of the calcium chloride aqueous solution ranges from 0.05 mol / L to 0.15 mol / L; The standing time is 16 to 20 hours.

7. The preparation method according to claim 1, characterized in that: In step S6, the volume percentage concentration of glutaraldehyde in the mixed solution is 2.0% to 4.0%; the concentration of hydrochloric acid in the mixed solution is 0.05 mol / L to 0.15 mol / L; The post-treatment B comprises: washing with ultrapure water until neutral, and placing in a cold dryer for cold drying.

8. A selective lead stabilizer for sodium alginate embedded in chitosan modified by thiosemicarbazide, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 7.

9. Use of the selective lead stabilizer of sodium alginate embedded in semicarbazide-modified chitosan according to claim 8 in the treatment of soil heavy metal pollution.

10. The use according to claim 9, characterized in that: include: The selective lead stabilizer of thiosemicarbazide-modified chitosan-embedded sodium alginate was uniformly applied to soil contaminated with heavy metals.

Citation Information

Cited By

  • Thiourea-tertiary amine bifunctional chitosan microsphere and preparation method thereof

    CN122076395A