Supercritical fluorine-containing polyimide foam and preparation method thereof

By simplifying the process and optimizing the treatment conditions, supercritical fluoropolyimide foam is prepared using copolyester ammonium precursor powder, which solves the problems of complex preparation and insufficient performance in the prior art, and achieves efficient and environmentally friendly industrial production and high performance materials applications.

CN119039652APending Publication Date: 2024-11-29CHANGZHOU TIANSHENG NEW MATERIALS RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411388841.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The preparation process of existing fluoropolyimide materials is complex and has a long reaction time, which cannot meet the needs of industrial scale production and application. At the same time, their temperature resistance and strength are poor.

Method used

The supercritical fluorinated polyimide foam is made by cold-pressed foaming and curing treatment. The appropriate solvent and supercritical fluid are selected using the combination of fluorinated dianhydride and fluorinated diamine. , optimize the pressing and curing treatment conditions, simplify the process and improve the reaction efficiency.

Benefits of technology

It realizes a green and environmentally friendly foaming process with simple process, short reaction time and high production efficiency, improves the mechanical properties and thermal stability of the foam, and is suitable for industrial scale production and high-performance applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of fluorine-containing polyimide foam, in particular to supercritical fluorine-containing polyimide foam and a preparation method thereof. The supercritical fluorine-containing polyimide foam is prepared by carrying out cold pressing on copolymerized polyester ammonium salt precursor powder, foaming and curing, wherein the copolymerized polyester ammonium salt precursor powder comprises the following substances in parts by weight: 8-15 parts of fluorine-containing dianhydride, 8-12 parts of fluorine-containing diamine and 3-12 parts of a solvent. The foaming ratio of the fluorine-containing polyimide foam prepared in the invention is 5-30 times, and the pore diameter of the foaming material is 100-300 [mu] m. The fluorine-containing polyimide foam prepared by the preparation method disclosed by the invention has relatively high high-temperature resistance and excellent mechanical properties. The compression performance at normal temperature and high temperature can be superior to that of PMI, and the use requirement of high-temperature bearing can be met. The preparation method is simple in preparation process, short in reaction time, easy to control, high in production efficiency, green and environment-friendly in foaming process, wide in application range and beneficial to industrial large-scale production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorine-containing polyimide foam, in particular to a supercritical fluorine-containing polyimide foam and a preparation method thereof. Background Art

[0002] As a newly developed new type of material, high temperature resistant foam materials have greatly promoted the development of science and technology and various industrial fields. In various high-tech industries, new requirements have been put forward for high-performance and high temperature resistant foam materials. In order to meet the higher requirements of the application field, broadening the application depth and width of foam materials has become one of the urgent issues for many R&D manufacturers and front-line researchers.

[0003] The existing commonly used polyurethane, rigid polyvinyl chloride, and methacrylic imide foam core materials have the defects of poor temperature resistance and core strength. Fluorinated polyimide is a type of polymer material with excellent performance. Its chemical structure contains fluorine elements, which makes it show special advantages in thermal stability, electrical insulation and chemical resistance. Polyimide itself is a high-performance polymer material, widely used in aerospace, electronics, medical and other fields. After adding fluorine elements, the performance of the material is significantly enhanced.

[0004] With respect to the above-mentioned related technologies, the inventors found that the existing preparation process of fluorinated polyimide is relatively complicated and the reaction time is relatively long, which cannot meet the needs of existing industrial-scale production and application. Summary of the invention

[0005] In order to improve the existing fluorinated polyimide materials, which have poor strength and temperature resistance and complex preparation process and long reaction time, the present application provides a supercritical fluorinated polyimide foam and a preparation method thereof.

[0006] In the first aspect, the present application provides a supercritical fluorinated polyimide foam, which adopts the following technical solution: A supercritical fluorine-containing polyimide foam is prepared by cold-pressing a copolymerized polyester ammonium salt precursor powder, foaming it and curing it. The copolymerized polyester ammonium salt precursor powder comprises the following materials in parts by weight: 8-15 parts of fluorine-containing dianhydride, 8-12 parts of fluorine-containing diamine, and 3-12 parts of a solvent.

[0007] Through the above technical scheme, the present application uses copolymerized polyester ammonium salt precursor powder as the main raw material, and is made by cold pressing foaming and curing treatment. The process is simple, the reaction time is short, it is easy to control, the production efficiency is high, and the foaming process is green and environmentally friendly, with a wide range of applications, which is conducive to realizing industrial-scale production and application.

[0008] At the same time, the selection of fluorinated dianhydride and fluorinated diamine in the technical solution of the present application ensures that the foam has good mechanical properties, good high temperature resistance and mechanical strength.

[0009] Further, the fluorine-containing diamine includes one or more of 4,4'-oxybis[3-(trifluoromethyl)aniline], 4,4'-oxybis[3-(oxytrifluoromethyl)aniline], 4,4'-oxybis[3-fluoroaniline], 2-(trifluoromethyl)-1,4-p-phenylenediamine, 2-(oxytrifluoromethyl)-1,4-p-phenylenediamine, 2-fluoro-1,4-p-phenylenediamine, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 2,2'-bis(oxytrifluoromethyl)diaminobiphenyl and 2,2'-bis(fluoro)diaminobiphenyl.

[0010] Through the above technical solution, this application optimizes the types of fluorinated diamines, so that the obtained polyimide foam has greater flexibility and adaptability in performance. Among them, compounds such as 4,4'-oxybis[3-(trifluoromethyl)aniline] provide higher heat resistance and strength, while 2-(trifluoromethyl)-1,4-p-phenylenediamine and the like may improve the toughness and elasticity of the foam. By combining different types of fluorinated diamines, the performance characteristics of the foam can be adjusted to meet specific application requirements, which has important practical value in the fields of materials science and engineering.

[0011] Furthermore, the solvent includes one or more of DMF, DMAC, NMP, and DMSO.

[0012] Through the above technical scheme, the present application optimizes the type of solvent and selects a suitable solvent system, which can not only improve the uniformity of the reaction, but also improve the solubility of the precursor powder, thereby forming a more uniform bubble structure during the foaming process, ensuring the physical properties, mechanical strength and thermal stability of the final product. In addition, the selection of environmentally friendly solvents can reduce the negative impact on the environment and meet the requirements of sustainable development.

[0013] Furthermore, the copolyester ammonium salt precursor powder is prepared by the following scheme: Adding fluorinated dianhydride and fluorinated diamine into a solvent, heating and keeping the temperature to react, and collecting a reaction liquid; The reaction solution is dried, ground and sieved to obtain copolymerized polyester ammonium salt precursor powder.

[0014] Through the above technical scheme, the present application can make the reaction more complete by adding fluorinated dianhydride and fluorinated diamine to the solvent for heating reaction, and the generated copolyester ammonium salt precursor powder has higher purity and better performance. The introduction of drying, grinding and screening steps ensures the uniformity of the particle size of the precursor powder, and the stability of the bubbles in the foaming process can be effectively improved through uniform particle distribution, and finally the density and structural strength of the foam are improved, thereby enhancing the mechanical properties and high temperature resistance of the fluorinated polyimide foam.

[0015] In the second aspect, the present application provides a method for preparing a supercritical fluorinated polyimide foam, using the following technical solution: A method for preparing a supercritical fluorinated polyimide foam comprises the following preparation steps: The ammonium salt precursor powder of the copolymerized polyester is placed in a mold and subjected to pressing treatment to prepare an ammonium salt precursor body of the copolymerized polyester; At a first temperature, placing a copolymerized polyester ammonium salt precursor embryo in a mold cavity, and filling a supercritical fluid to equilibrium to obtain a polymer-supercritical fluid homogeneous system; After maintaining the pressure of the polymer-supercritical fluid homogeneous system obtained in the above step stable, heating to a second temperature, releasing the pressure and foaming to obtain a supercritical fluorinated polyimide foamed embryo plate; The supercritical fluorinated polyimide foam can be prepared by placing the supercritical fluorinated polyimide foamed embryo plate in a high temperature environment for curing.

[0016] Through the above technical scheme, the present application optimizes the production process of supercritical fluorinated polyimide foam. First, through the pressing process, the density and uniformity of the precursor material are ensured. Then, through the introduction of supercritical fluid, a homogeneous system is formed, which avoids the defects in the preparation of traditional foams and improves the overall performance of the foam. Finally, after high-temperature curing treatment, the degree of chemical crosslinking of the foam is ensured, thereby improving its mechanical properties and thermal stability, which meets the high-demand application scenarios.

[0017] Furthermore, the pressing process is performed at a pressure of 10-20 MPa for 3-8 hours.

[0018] Through the above technical scheme, the present application optimizes the pressure of the pressing treatment and carries out the pressing treatment under appropriate pressure and time, which can effectively remove bubbles and voids in the material and improve the density of the precursor, thereby improving the uniformity and structural stability of the foam in the subsequent foaming process, and greatly improving the mechanical properties and durability of the final product.

[0019] Furthermore, the curing treatment is carried out at a temperature of 230-250° C. for 3-5 hours.

[0020] Through the above technical solution, the present application optimizes the curing temperature, and by adjusting the curing temperature and time, improves the cross-linking degree of the polyimide chain, thereby improving the thermal stability and mechanical properties of the foam. A moderate curing time can enable the material to form a more stable three-dimensional network structure, thereby improving the mechanical strength and chemical corrosion resistance of the foam. In addition, this temperature range also ensures that thermal degradation of the material does not occur, providing greater safety and reliability for the application of the foam.

[0021] Furthermore, the first temperature is not higher than the second temperature, the first temperature is 150-180°C and the second temperature is 180-200°C.

[0022] Through the above technical solution, the application ensures the smooth progress of the supercritical fluid treatment process by setting a reasonable interval between the first temperature and the second temperature. First, a homogeneous system is formed at a low temperature of 150-180°C, which can effectively avoid premature expansion of the foam, thereby increasing the stability of the foam and reducing the defect rate. Further foaming at a high temperature of 180-200°C can promote the rapid expansion and molding of the polymer, forming an ideal foam structure to meet the requirements of high-performance materials.

[0023] Furthermore, the supercritical fluid comprises supercritical N 2 and / or supercritical CO 2 The pressure of the supercritical fluid is 7.2~20MPa; the time for filling the supercritical fluid to equilibrium is 30~60min, the time for heating to the second temperature is 20~30min, and the temperature is maintained for 5~30min after heating to the second temperature.

[0024] Through the above technical solution, the present application uses supercritical fluid to significantly improve the efficiency and effect of the foaming process, ensures that the physical and chemical properties of the fluid are utilized during the reaction process, and promotes the formation and stability of bubbles. The specified filling time and heating time ensure the uniformity and controllability of the reaction process, and ultimately improves the performance and quality of the foam.

[0025] Furthermore, the pressure relief pressure after the pressure relief foaming is normal pressure, and the pressure relief rate is 10-100 MPa / s.

[0026] Through the above technical solution, the present application can ensure the instantaneous expansion of the foam through a reasonable pressure relief rate, form a fine and uniform foam structure, avoid the rupture and uneven distribution of bubbles, and thus improve the physical properties and appearance quality of the final product. In addition, controlling the pressure relief rate also helps to reduce stress concentration, improve the durability and structural stability of the material, and expand its application range.

[0027] In summary, this application has the following beneficial effects: First, the present application uses copolymerized polyester ammonium salt precursor powder as the main raw material, and is made by cold-pressing foaming and curing treatment. The process is simple, the reaction time is short, it is easy to control, the production efficiency is high, and the foaming process is green and environmentally friendly, with a wide range of applications, which is conducive to the realization of industrial-scale production and application.

[0028] Second, the present application uses copolymerized polyester ammonium salt precursor powder as the main raw material, which is made by cold-pressing foaming and curing treatment. The process is simple, the reaction time is short, it is easy to control, and the production efficiency is high. Moreover, the foaming process is green and environmentally friendly, and has a wide range of applications, which is conducive to realizing industrial-scale production and application.

[0029] Third, this application optimizes the production process of supercritical fluorinated polyimide foam. First, through the pressing process, the density and uniformity of the precursor material are ensured. Then, through the introduction of supercritical fluid, a homogeneous system is formed, which avoids the defects in traditional foam preparation and improves the overall performance of the foam. Finally, after high-temperature curing treatment, the degree of chemical cross-linking of the foam is ensured, thereby improving its mechanical properties and thermal stability, which meets the high-demand application scenarios. DETAILED DESCRIPTION

[0030] The present application is further described in detail below with reference to the embodiments.

[0031] In the examples of the present application, the raw materials and instruments used are as follows, but not limited thereto. Raw materials not otherwise specified are of analytical grade.

[0032] Preparation Example 1 444 g of hexafluorodianhydride and 428 g of 4,4'-oxybis[3-(trifluoromethyl)aniline] were reacted in 300 g of DMF at 80° C. for 5 h to obtain a copolymerized polyester ammonium salt precursor solution, which was then dried, ground, and screened to obtain a copolymerized polyester ammonium salt precursor powder 1.

[0033] Preparation Example 2 444 g of hexafluorodianhydride and 108 g of 2-(trifluoromethyl)-1,4-p-phenylenediamine were reacted in 400 g of DMAC at 90° C. for 5 h to obtain a copolymerized polyester ammonium salt precursor solution, which was then dried, ground, and screened to obtain a copolymerized polyester ammonium salt precursor powder 2.

[0034] Preparation Example 3 444 g of hexafluorodianhydride and 320 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl were reacted in 400 g of DMF at 90° C. for 4 h to obtain a copolymerized polyester ammonium salt precursor solution, which was then dried, ground, and screened to obtain a copolymerized polyester ammonium salt precursor powder 3.

[0035] Example 1 A method for preparing a supercritical fluorinated polyimide foam comprises the following preparation steps: The copolymerized polyester ammonium salt precursor powder 1 is placed in a mold, the pressure in the press is controlled to be 20 MPa, and the pressing treatment is performed for 4 hours to prepare a copolymerized polyester ammonium salt precursor green body; The ammonium salt precursor of the copolymerized polyester is placed in a mold cavity at 160°C, and carbon dioxide is filled into the mold cavity until the mold cavity reaches a supercritical state. The pressure is controlled at 12 MPa, and the pressure is maintained for 30 minutes to obtain a polymer-supercritical fluid homogeneous system. After maintaining the pressure of the polymer-supercritical fluid homogeneous system obtained in the above steps stable, the temperature is raised to 185° C., and the pressure is supplemented by a booster pump to maintain the pressure in the mold cavity at 15 MPa for 30 minutes. The pressure is then released by a pneumatic ball valve to release the pressure in the mold cavity from 15 MPa to 0 (normal pressure). The pressure relief rate is controlled between 20 and 50 MPa / s by adjusting the diameter of the pneumatic ball valve. The mold cavity is opened to obtain a foamed blank, which is then post-cured in an oven at 230° C. for 5 hours to obtain a fluorinated polyimide foam, thereby preparing the supercritical fluorinated polyimide foam.

[0036] Example 2 A method for preparing a supercritical fluorinated polyimide foam comprises the following preparation steps: The copolymerized polyester ammonium salt precursor powder 2 is placed in a mold, the pressure in the press is controlled to be 18 MPa, and the pressing treatment is performed for 5 hours to prepare a copolymerized polyester ammonium salt precursor green body; The ammonium salt precursor of the copolymerized polyester is placed in a mold cavity at 165°C, and carbon dioxide is filled into the mold cavity until the supercritical state is reached. The pressure is controlled at 13 MPa, and the pressure is maintained for 35 minutes to obtain a polymer-supercritical fluid homogeneous system. After maintaining the pressure of the polymer-supercritical fluid homogeneous system obtained in the above steps stable, the temperature is raised to 190° C., and the pressure is supplemented by a booster pump to maintain the pressure in the mold cavity at 15 MPa for 30 minutes. The pressure is then released by a pneumatic ball valve to release the pressure in the mold cavity from 15 MPa to 0 (normal pressure). The pressure relief rate is controlled between 20 and 50 MPa / s by adjusting the diameter of the pneumatic ball valve. The mold cavity is opened to obtain a foamed blank, which is then post-cured in an oven at 250° C. for 4 hours to obtain a fluorinated polyimide foam, thereby preparing the supercritical fluorinated polyimide foam.

[0037] Example 3 A method for preparing a supercritical fluorinated polyimide foam comprises the following preparation steps: The copolymerized polyester ammonium salt precursor powder 3 was placed in a mold, and the pressure in the press was controlled to be 20 MPa, and the pressing process was performed for 4 hours to prepare a copolymerized polyester ammonium salt precursor green body; The ammonium salt precursor of the copolymerized polyester is placed in a mold cavity at 170°C, and carbon dioxide is filled into the mold cavity until the mold cavity reaches a supercritical state. The pressure is controlled at 14 MPa, and the pressure is maintained for 30 minutes to obtain a polymer-supercritical fluid homogeneous system. After maintaining the pressure of the polymer-supercritical fluid homogeneous system obtained in the above steps stable, the temperature is raised to 195°C, and the pressure is supplemented by a booster pump to maintain the pressure in the mold cavity at 15MPa for 35 minutes. The pressure is then released by a pneumatic ball valve to release the pressure in the mold cavity from 15MPa to 0 (normal pressure). The pressure relief rate is controlled between 20 and 50MPa / s by adjusting the diameter of the pneumatic ball valve. The mold cavity is opened to obtain a foamed blank, which is then post-cured in an oven at 245°C for 4 hours to obtain a fluorinated polyimide foam, thereby preparing the supercritical fluorinated polyimide foam.

[0038] Comparative Example In a three-necked flask equipped with a mechanical stirrer, a thermometer, and a reflux condenser, 36.6 g (0.1 mol) of 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane dissolved in N,N'-dimethylformamide (DMF), 42.7 g (0.1 mol) of 1,4-difluoropyromellitic dianhydride, and 1.6 g (0.01 mol) of a capping agent 5-norbornene-2,3-dicarboxylic anhydride were added in order according to the ratio. The cooling liquid was circulated under stirring to maintain the reaction at 10°C for condensation reaction. The total condensation reaction took about 6.5 hours. ; The system was heated to 20°C, and an organic base 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) was added to neutralize the system to a pH value of 6.5; the resin system was dehydrated under reduced pressure at a vacuum degree of 0.081 MPa and a temperature of 60°C in a water bath until the viscosity reached 5800 mPa.s, and the dehydration was stopped. The system was cooled to 50°C and discharged to obtain a fluorinated polyimide C. 100 parts by weight of the fluorinated polyimide C was rapidly foamed under a microwave condition of 700 W for 10 minutes, and the system was placed at room temperature for 2 hours for post-curing to prepare a fluorinated polyimide foam.

[0039] Performance Testing The supercritical fluorinated polyimide foams prepared in Examples 1-3 and the fluorinated polyimide foams prepared in the comparative example were subjected to performance tests: Performance test standard: according to DB51 / T 2683-2020 standard; The results are shown in Table 1 below: Table 1 Performance test table

[0040] From the above examples 1-3 and the comparative example, combined with the test results in Table 1, it can be found that: From the comparison between Examples 1-3 and the comparative example, it is shown that the technical solution of the present application optimizes the production process of supercritical fluorinated polyimide foam. First, the compactness and uniformity of the precursor material are ensured by pressing. Then, a homogeneous system is formed by introducing a supercritical fluid, thereby avoiding the defects in the preparation of traditional foams and improving the overall performance of the foam. Finally, after high-temperature curing treatment, the degree of chemical crosslinking of the foam is ensured, thereby improving its mechanical properties and thermal stability.

[0041] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0042] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.

[0043] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0044] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.

Claims

1. A supercritical fluorinated polyimide foam, It is characterized in that The copolyester ammonium salt precursor powder is cold pressed, foamed and solidified, and the copolyester ammonium salt precursor powder includes the following materials in parts by weight: 8-15 parts of fluorinated dianhydride; 8-12 parts of fluorinated diamine; 3-12 parts of solvent.

2. A supercritical fluorinated polyimide foam according to claim 1, It is characterized in that The fluorine-containing diamine includes one or more of 4,4'-oxybis[3-(trifluoromethyl)aniline], 4,4'-oxybis[3-(oxytrifluoromethyl)aniline], 4,4'-oxybis[3-fluoroaniline], 2-(trifluoromethyl)-1,4-p-phenylenediamine, 2-(oxytrifluoromethyl)-1,4-p-phenylenediamine, 2-fluoro-1,4-p-phenylenediamine, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 2,2'-bis(oxytrifluoromethyl)diaminobiphenyl and 2,2'-bis(fluoro)diaminobiphenyl.

3. The supercritical fluorinated polyimide foam according to claim 1, It is characterized in that The solvent includes one or more of DMF, DMAC, NMP and DMSO.

4. The supercritical fluorinated polyimide foam according to claim 1, It is characterized in that The copolyester ammonium salt precursor powder is prepared by the following scheme: Adding fluorinated dianhydride and fluorinated diamine into a solvent, heating and keeping the temperature to react, and collecting a reaction liquid; The reaction solution is dried, ground and sieved to obtain copolymerized polyester ammonium salt precursor powder.

5. A method for preparing a supercritical fluorinated polyimide foam according to any one of claims 1 to 4, It is characterized in that The method comprises the following preparation steps: The ammonium salt precursor powder of the copolymerized polyester is placed in a mold and subjected to pressing treatment to prepare an ammonium salt precursor body of the copolymerized polyester; At a first temperature, placing a copolymerized polyester ammonium salt precursor embryo in a mold cavity, and filling a supercritical fluid to equilibrium to obtain a polymer-supercritical fluid homogeneous system; After maintaining the pressure of the polymer-supercritical fluid homogeneous system obtained in the above step stable, heating to a second temperature, releasing the pressure and foaming to obtain a supercritical fluorinated polyimide foamed embryo plate; The supercritical fluorinated polyimide foam can be prepared by placing the supercritical fluorinated polyimide foamed embryo plate in a high temperature environment for curing.

6. The method for preparing a supercritical fluorinated polyimide foam according to claim 5, It is characterized in that The pressing process is performed at a pressure of 10-20 MPa for 3-8 hours.

7. The method for preparing a supercritical fluorinated polyimide foam according to claim 5, It is characterized in that The curing treatment is carried out at a temperature of 230-250° C. for 3-5 hours.

8. The method for preparing a supercritical fluorinated polyimide foam according to claim 5, It is characterized in that The first temperature is not higher than the second temperature, the first temperature is 150-180°C and the second temperature is 180-200°C.

9. The method for preparing a supercritical fluorinated polyimide foam according to claim 5, It is characterized in that The supercritical fluid includes supercritical N 2 and / or supercritical CO 2 The pressure of the supercritical fluid is 7.2~20MPa; the time for filling the supercritical fluid to equilibrium is 30~60min, the time for heating to the second temperature is 20~30min, and the temperature is maintained for 5~30min after heating to the second temperature.

10. The method for preparing a supercritical fluorinated polyimide foam according to claim 5, It is characterized in that The pressure relief pressure after the pressure relief foaming is normal pressure, and the pressure relief rate is 10-100 MPa / s.

Citation Information

Cited By

  • Supercritical polyimide foam and preparation method thereof

    CN122167810A