Millimeter-scale calcium alginate gel ball with open macroporous structure and preparation method of millimeter-scale calcium alginate gel ball
By using CO2 gas to form a connecting macroporous structure during the preparation process of calcium alginate gel balls and forming an open pore structure through etchant, the problem that calcium alginate gel balls is difficult to obtain open macropores is solved, and the problem is improved. Adsorption and growth environment of cells in three-dimensional culture in vitro.
Patent Information
- Application Number
- CN202411177792.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The prior art is difficult to obtain open macroporous structures when preparing calcium alginate gel spheres, resulting in poor adsorption and growth of cells in three-dimensional cultures in vitro.
Sodium alginate, pore-generating agent and water-soluble anionic surfactant are used to dissolve in water to form a gel precursor solution, and drip it into a calcium ions-containing coagulation bath solution to form a connecting macroporous structure, and then An open pore structure was formed using an etchant to obtain a millimeter-scale calcium alginate gel ball with open macropores.
The micron-scale pore structure connected to each other inside the calcium alginate gel sphere is realized, which shortens the transmission distance between cells and nutrients, improves the cell adsorption and growth environment, and ensures the uniform dispersion and functional expression of cells.
Smart Images

Figure HDA0005011206550000011 
Figure HDA0005011206550000012 
Figure HDA0005011206550000013
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedicine and relates to millimeter-scale calcium alginate gel spheres with an open macroporous structure and a preparation method thereof. Background Art
[0002] The growth of tissues and cells in the body is based on the in vivo environment. Traditional two-dimensional cell culture can only provide balanced nutrients for each cell. The cell morphology is very different from that in the body and cannot simulate in vivo differentiation and gene expression. As an emerging in vitro cell culture technology, three-dimensional cell culture can provide cells with a three-dimensional growth space, promote their growth, proliferation and migration, and the cell morphology is closer to the natural growth morphology. Three-dimensional cell culture technology combines the advantages of in vitro two-dimensional cell culture and in vivo models to form a convenient and efficient research system, and can provide an important platform for drug screening, disease treatment and tissue engineering.
[0003] With the continuous development of biomaterials, more and more scaffold materials are used for in vitro three-dimensional cell culture. The forms of scaffold materials used for three-dimensional cell culture include hydrogels, fibers, porous structure scaffolds, and 3D printed scaffolds. The structure of traditional macroporous scaffolds is generally large. Although macropores can be used to enhance the delivery of nutrients, the large structure of macroporous scaffolds will lead to excessive delivery distances. Therefore, some researchers combined the macroporous structure with the microsphere structure and proposed macroporous gel balls. Macroporous gel balls have a high specific surface area, which is conducive to cell growth, proliferation, differentiation and expression, etc., can enhance the delivery of nutrients and oxygen to cells, and are also conducive to the timely discharge of metabolic waste from cells. The open and connected pores of macroporous gel balls are also conducive to the formation of cell-cell and cell-extracellular matrix (ECM) interactions. Therefore, macroporous gel balls have received widespread attention from researchers. In three-dimensional cell culture, the pore size, porosity, and whether the pores are connected of macroporous gel balls have a great influence on cell adhesion, growth, migration, proliferation, differentiation, and protein expression.
[0004] Sodium alginate (NaAlg) is an anionic polysaccharide composed of β-D-mannuronic acid (M) and α-L-guluronic acid (G), which can form alginate hydrogels with multivalent cations. Alginate hydrogels are widely used as cell microcarrier materials due to their good biocompatibility, biodegradability and bioadhesion. The preparation of cell-loaded alginate gel balls can be divided into pre-loading cell method and post-loading cell method. The pre-loading cell method requires stirring the cell suspension to mix it with the target solution. The cells will be subjected to fluid shear force. During the preparation process, the cells may also come into contact with slightly toxic reagents, surfactants, etc., and sometimes ultraviolet curing is required. These factors will cause certain damage to the cells. The post-loading cell method can avoid these adverse effects and load the cells into the interior of the gel ball without loss. The post-loading cell method requires that the outer side of the alginate gel ball has larger holes to facilitate the entry of cells into the interior of the gel ball. However, in the process of preparing calcium alginate gel balls, due to the interaction between alginate and Ca 2+ The cross-linking speed is too fast, and it is difficult to obtain open pores. Currently, there are still great challenges in preparing calcium alginate gel spheres with open interconnected macroporous structures.
[0005] For example, Quraishi et al. fully contacted an aqueous solution of alginate containing lignin and calcium carbonate with carbon dioxide bubbles under low pressure, and after the bubbles stopped generating, the solution was transferred to an ethanol solution for supercritical drying to prepare a calcium alginate scaffold, see Quraishi S., Martins M., Barros AA, et al. L. Novel non-cytotoxic alginate–lignin hybrid aerogels as scaffolds for tissue engineering [J]. The Journal of Supercritical Fluids, 2015, 105: 1-8. Although the scaffold has structural and morphological characteristics suitable for tissue engineering applications, its overall structure is relatively large, with a scaffold size of 10 mm, and its pore structure is mostly composed of holes of about 1 μm, which is too small to be conducive to cell adsorption into the scaffold. Summary of the invention
[0006] In view of the problem that it is difficult to obtain an open macroporous structure when preparing calcium alginate gel balls in the prior art, the present invention provides a millimeter-sized calcium alginate gel ball with an open macroporous structure and a preparation method thereof, so as to realize the preparation of alginate gel balls with both an open interconnected macroporous structure and a millimeter-sized small size.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0008] A millimeter-scale calcium alginate gel ball with an open macroporous structure, wherein the matrix material of the gel ball is calcium alginate, the interior of the gel ball has an interconnected micrometer-scale pore structure, and the interconnected micrometer-scale pore structure inside the gel ball is opened on the surface of the gel ball, the average pore size of the micrometer-scale pore structure inside the gel ball is 120-160 μm, and the particle size of the gel ball when reaching swelling equilibrium in water is 2-5 mm.
[0009] In the technical solution of the above-mentioned millimeter-scale calcium alginate gel ball with an open macroporous structure, the average pore size of the pore structure on the surface of the gel ball is 150-200 μm, and further, the porosity of the pore structure on the surface of the gel ball is 20%-40%.
[0010] Furthermore, in the technical solution of the above-mentioned millimeter-sized calcium alginate gel sphere with an open macroporous structure, the porosity of the pore structure inside the gel sphere is 50% to 70%.
[0011] The present invention also provides a method for preparing the above-mentioned millimeter-sized calcium alginate gel spheres with an open macroporous structure, comprising the following steps:
[0012] (1) dissolving sodium alginate, a porogen and a water-soluble anionic surfactant in water, homogenizing and emulsifying the resulting mixed solution to incorporate bubbles into the mixed solution, and obtaining a gel precursor solution; in the gel precursor solution, the concentration of sodium alginate is 1.5wt% to 2wt%, the concentration of the porogen is 1wt% to 2wt%, and the concentration of the water-soluble anionic surfactant is 0.05wt% to 0.15wt%; the porogen is sodium bicarbonate or potassium bicarbonate;
[0013] Dissolving a water-soluble calcium salt and glacial acetic acid in water to obtain a coagulation bath solution, wherein the concentration of the water-soluble calcium salt in the coagulation bath solution is 5wt% to 15wt%, and the concentration of the glacial acetic acid is 5wt% to 15wt%;
[0014] (2) dripping a gel precursor into a coagulation bath solution through an injection needle, wherein the sodium alginate in the gel precursor droplets dripping into the coagulation bath solution undergoes a cross-linking reaction with calcium ions, and at the same time, the porogen in the gel precursor droplets dripping into the coagulation bath solution reacts with glacial acetic acid to generate CO2 gas in the gel precursor droplets, thereby connecting bubbles in the gel precursor droplets, and after the gel precursor droplets are cross-linked to solidify, the solid-liquid separation is performed, and the unreacted water-soluble calcium salt and glacial acetic acid in the obtained solid phase are removed by washing, and freeze-drying is performed to obtain millimeter-sized calcium alginate gel spheres having interconnected macropores inside;
[0015] (3) immersing the gel ball obtained in step (2) in an etchant aqueous solution, etching under stirring, so that the etchant is complexed with the calcium ions in the calcium alginate on the surface of the gel ball to form an open-pore structure on the surface of the gel ball, immediately replacing the etchant aqueous solution with water to terminate the reaction between the etchant and the calcium ions, separating the solid and the liquid, washing and drying the obtained solid phase, and obtaining the etchant; the etchant is potassium citrate or sodium citrate, and the concentration of the etchant aqueous solution is 10 to 15 g / L.
[0016] In step (3) of the technical solution of the above preparation method, the etching time is preferably controlled to be 3 to 10 minutes.
[0017] In step (2) of the technical solution of the above preparation method, the gel precursor solution is preferably dripped into the coagulation bath solution through an injection needle with an inner diameter of 0.5 to 1 mm.
[0018] In step (2) of the technical solution of the above preparation method, the gel precursor solution is dripped into the coagulation bath solution through the injection needle at a flow rate of 15 to 25 mL / h from the injection pump.
[0019] In step (2) of the technical solution of the above preparation method, the cross-linking time should ensure that the gel precursor droplets are completely cross-linked and solidified, and the cross-linking time can usually be controlled to be 10 to 15 hours.
[0020] In step (1) of the technical solution of the above preparation method, the feasible water-soluble anionic surfactant may be sodium dodecyl sulfate or other water-soluble anionic surfactants.
[0021] The design concept of the present invention is mainly as follows:
[0022] The present invention provides a new strategy for preparing millimeter-sized calcium alginate (CaAlg) gel spheres with an open macroporous structure. First, sodium alginate (NaAlg), a porogen and a water-soluble anionic surfactant are dissolved in water, and then a gas is added to the obtained mixed solution by a homogenization emulsification method to form a mixed solution containing bubbles, i.e., a gel precursor solution. Due to the presence of the water-soluble anionic surfactant and the relatively high viscosity NaAlg, the bubbles in the gel precursor solution can exist stably. After the gel precursor solution is dropped into a coagulation bath solution containing a water-soluble calcium salt and glacial acetic acid, the NaAlg in the gel precursor solution droplets reacts with the CaAlg to form a mixed solution containing bubbles. 2+The cross-linking reaction occurs and the gel precursor droplets gradually solidify. At the same time, the porogen reacts with glacial acetic acid to produce a large amount of CO2 gas. The production of CO2 gas can promote the rapid nucleation and growth of bubbles inside the gel precursor droplets, and cause the bubbles in the gel precursor droplets to become connected. After the cross-linking is complete, millimeter-scale CaAlg gel balls with connected macropores inside (macroporous CaAlg gel balls) are obtained. The macroporous CaAlg gel balls are immersed in an etchant aqueous solution. During the immersion process, the anions of the etchant will compete with the alginate for Ca 2+ The CaAlg gel is transformed into a sol by complexing the etchant type, etchant solution concentration and etching time. 2+ The complexation reaction mainly occurs on the surface of the macroporous CaAlg gel sphere, and then an open-pore structure is formed on the surface of the macroporous CaAlg gel sphere, that is, the pore structure that is interconnected inside the macroporous CaAlg gel sphere is opened on the surface of the gel sphere, thereby obtaining a millimeter-scale CaAlg gel sphere with an open macroporous structure.
[0023] Compared with the prior art, the technical solution of the present invention produces the following beneficial technical effects:
[0024] 1. The present invention provides a millimeter-scale calcium alginate gel ball with an open macroporous structure, wherein the interior of the gel ball has a micron-scale pore structure that interpenetrates each other, and the micron-scale pore structure that interpenetrates each other inside the gel ball is opened on the surface of the gel ball, and the particle size of the gel ball when it reaches swelling equilibrium in water is 2 to 5 mm. When the gel ball of the present invention is used for in vitro 3D cell culture, this interpenetrating open pore structure and relatively small gel ball size are conducive to cell adsorption and uniform dispersion. When the cell suspension is dripped onto the gel ball, the cells can easily diffuse into the interior of the gel ball through the interpenetrating open pores and disperse evenly, which is conducive to the material exchange between the cell and the external environment. It is a macroporous gel ball scaffold with good biocompatibility and convenient for cell transfer and culture. Compared with the existing calcium alginate porous scaffolds with large size and small pore structure, the reduction of the size of the gel ball of the present invention is conducive to shortening the transmission distance of the material, and the increase of the pores inside and on the surface of the gel ball of the present invention (the average pore size is above 100 μm) is more conducive to cell adsorption into the interior of the gel ball.
[0025] 2. The present invention has confirmed through cell adsorption experiments that, compared with gel balls with interconnected macroporous structures inside but without open pore structures on the surface, the millimeter-scale calcium alginate gel balls with open macroporous structures described in the present invention can more evenly adsorb HepG2 cells.
[0026] 3. The present invention has confirmed through the activity and proliferation experiments of HepG2 cells that the millimeter-sized calcium alginate gel spheres with open macroporous structure of the present invention can provide a good environment for cell growth and proliferation, and the cells grow in clusters inside the gel spheres. After culturing for 24h, 48h and 72h, the activity of HepG2 cells is above 95%, and the number of cells after culturing for 48h and 72h is 1.4 times and 2.3 times that of the cells after culturing for 24h, which can ensure the normal growth and proliferation of cells.
[0027] 4. The present invention confirms through in vitro secretion experiments of HepG2 cells that the millimeter-scale calcium alginate gel spheres with an open macroporous structure of the present invention can maintain the functional expression of cells.
[0028] 5. The present invention also provides a method for preparing the above-mentioned millimeter-sized calcium alginate gel spheres with an open macroporous structure. The method comprises adding air bubbles into the gel precursor solution, and in the process of cross-linking sodium alginate and calcium ions, an etchant and glacial acetic acid are used to form an interconnected macroporous structure in the cross-linked and solidified gel spheres to obtain macroporous calcium alginate gel spheres. On this basis, the etchant is combined with calcium ions in the surface layer of the macroporous calcium alginate gel spheres to form an open-pore structure on the surface of the macroporous calcium alginate gel spheres. This solves the problem of the prior art that alginic acid and calcium ions are not easily oxidized. 2+ The cross-linking speed is too fast, making it difficult to obtain open pores. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a scanning electron microscope image of the macroporous CaAlg gel spheres prepared in step (2) of Example 1.
[0030] Figure 2 These are optical photographs of macroporous CaAlg gel spheres prepared in four groups of experiments in Example 2.
[0031] Figure 3 These are optical photographs of the four gel precursor solutions in Example 3 after being placed for different periods of time.
[0032] Figure 4 These are optical photographs of macroporous CaAlg gel spheres prepared in four groups of experiments in Example 3.
[0033] Figure 5 This is a scanning electron microscope image of the cross section of the macroporous CaAlg gel spheres prepared in the four groups of experiments in Example 3.
[0034] Figure 6 This is an optical photograph of macroporous CaAlg gel spheres prepared by 4 groups of experiments in Example 4.
[0035] Figure 7 This is a scanning electron microscope image of the macroporous CaAlg gel spheres prepared in the four groups of experiments in Example 4.
[0036] Figure 8 This is an optical photograph of the macroporous CaAlg gel sphere during the etching process in Example 5.
[0037] Fig. 9 3 is a scanning electron microscope image of the open-pore CaAlg gel spheres obtained by etching for different times in Example 5.
[0038] Fig.10 It is a scanning electron microscope image of the open-pore CaAlg gel spheres prepared in each group of experiments when potassium citrate is used as an etchant in Example 5.
[0039] Fig.11 These are the fluorescence images of the macroporous CaAlg gel spheres (a and b) and open-pore CaAlg gel spheres (c and d) after adsorption of HepG2 cells in Example 6, wherein a and c are bright fields, and b and d are fluorescence fields; the scale is 500 μm.
[0040] Fig.12 This is the result of observing the activity of HepG2 cells using the live-dead cell staining method in Example 7. In the figure, UGS represents macroporous CaAlg gel spheres, and OGS represents open-pore CaAlg gel spheres.
[0041] Fig.13 Figures a and b are the cell activity test results of the open-pore CaAlg gel balls in Example 7 after culturing HepG2 cells for 24h, 48h and 72h, as well as the cell proliferation of HepG2 cells after culturing the macroporous CaAlg gel balls and the open-pore CaAlg gel balls for 24h, 48h and 72h, respectively; in the figures, General porous represents macroporous CaAlg gel balls, and Open porous represents open-pore CaAlg gel balls.
[0042] Fig.14 Figures a and b show the OD value and urea concentration of urea in the supernatant after culturing HepG2 cells for different time periods using macroporous CaAlg gel balls and open porous CaAlg gel balls in Example 8, respectively. In the figure, General porous represents macroporous CaAlg gel balls, and Open porous represents open porous CaAlg gel balls.
[0043] Fig.15 Figures a and b show the OD value and CYP450 concentration of CYP450 in the supernatant after culturing HepG2 cells for different time periods using macroporous CaAlg gel balls and open-porous CaAlg gel balls in Example 8, respectively. In the figure, General porous represents macroporous CaAlg gel balls, and Open porous represents open-porous CaAlg gel balls. DETAILED DESCRIPTION
[0044] The millimeter-sized calcium alginate gel spheres with an open macroporous structure and the preparation method thereof provided by the present invention are further illustrated by the following examples, which should not be construed as limiting the scope of protection of the present invention. Those skilled in the art may make some non-essential improvements and adjustments to the present invention based on the above-mentioned invention content, which still fall within the scope of protection of the present invention.
[0045] Example 1
[0046] In this embodiment, millimeter-sized calcium alginate (CaAlg) gel spheres with an open macroporous structure are prepared in the following steps:
[0047] (1) Sodium alginate (NaAlg) is dissolved in deionized water, and then sodium bicarbonate (NaHCO3) and sodium dodecyl sulfate (SDS) are added and stirred until NaHCO3 and SDS are completely dissolved. The resulting mixed solution is homogenized and emulsified in a homogenizer at a speed of 19000 rpm in an air atmosphere for 30 seconds to incorporate bubbles into the mixed solution to obtain a gel precursor solution; in the gel precursor solution, the concentration of NaAlg is 1.5wt%, the concentration of NaHCO3 is 1.5wt%, and the concentration of SDS is 0.1wt%.
[0048] Calcium chloride and glacial acetic acid (HAc) were dissolved in deionized water to obtain a coagulation bath solution, wherein the concentration of calcium chloride in the coagulation bath solution was 10 wt % and the concentration of HAc was 10 wt %.
[0049] (2) The gel precursor solution was transferred to a 20 mL syringe with a flat needle of 0.52 mm (model 21G) in inner diameter. The syringe was pushed vertically downward at a flow rate of 20 mL / h using a syringe pump. The gel precursor solution naturally dripped into the 150 mL coagulation bath solution through the needle of the syringe. The NaAlg in the formed gel precursor droplets reacted with the Ca in the coagulation bath. 2+ A cross-linking reaction occurs, and at the same time, NaHCO3 in the gel precursor droplets reacts with HAc in the coagulation bath to produce a large amount of CO2. The produced CO2 promotes the rapid nucleation and growth of bubbles in the gel precursor droplets, causing the bubbles in the gel precursor droplets to be connected. After 12 hours of cross-linking reaction, the gel precursor droplets solidify and the solid-liquid is separated. The obtained solid phase is washed with deionized water for 2 to 3 times to remove unreacted calcium chloride and HAc, and freeze-dried to obtain millimeter-scale CaAlg gel spheres with interconnected macropores inside (referred to as macroporous CaAlg gel spheres).
[0050] (3) The macroporous CaAlg gel spheres were added to a 15 g / L potassium citrate aqueous solution at a ratio of 4 g per 1 L potassium citrate aqueous solution, and the etching was carried out at a stirring speed of 20 rpm for 5 min. During the etching process, the citrate ions competed with the alginate ions for the Ca2+ The complexation of citrate and Ca 2+ After complexation, the outer layer of the macroporous CaAlg gel sphere is transformed into a sol state, and an open-pore structure is formed on the surface of the gel sphere. After etching, the potassium citrate solution is immediately absorbed and a large amount of deionized water is added to terminate the reaction. The solid-liquid separation is performed, and the obtained solid phase is washed with deionized water for 2 to 3 times and dried to obtain millimeter-scale CaAlg gel spheres with an open macroporous structure (referred to as open-pore CaAlg gel spheres).
[0051] The scanning electron microscope image of the macroporous CaAlg gel sphere prepared in step (2) of this embodiment is as follows: Figure 1 As shown, Figures a1 and a2 show the whole gel ball and the cut gel ball. Figure 1 The scale in the figure is 1 mm. Figure 1 It can be seen that the macroporous CaAlg gel spheres prepared in step (2) have interconnected pores inside, and the pore sizes are relatively uniform, but no pores are formed on the surface. This is because the Ca 2+ During the diffusion process, it first contacts the outer layer of the gel precursor droplet and rapidly undergoes a cross-linking reaction to generate CaAlg. The CaAlg formed on the outer layer of the gel precursor droplet encapsulates the CO2 bubbles generated by the reaction of NaHCO3 and HAc inside, thus failing to form a pore structure on the surface of the gel ball, and failing to obtain millimeter-scale CaAlg gel balls with an open macroporous structure.
[0052] The scanning electron microscope image of the open-pore CaAlg gel sphere prepared in step (3) of this example is as follows: Fig.10 As shown in Figure c3, it can be seen from the figure that after the etching operation in step (3), a relatively uniformly distributed open pore structure is formed on the surface of the gel ball, and a millimeter-scale CaAlg gel ball with an open macroporous structure is obtained.
[0053] Example 2
[0054] In this embodiment, syringe needles with different inner diameters were used to prepare millimeter-sized CaAlg gel spheres with an open macroporous structure.
[0055] In this embodiment, a total of 4 groups of experiments were set up. The operation of each group of experiments was basically the same as that of Example 1, except that the inner diameters of the flat-blade needles used in step (2) of each experimental group were 0.26 mm (model 25G), 0.42 mm (model 22G), 0.52 mm (model 21G) and 0.61 mm (model 20G), respectively.
[0056] Figure 2These are optical photographs of millimeter-sized CaAlg gel balls with interconnected macropores (referred to as macroporous CaAlg gel balls) prepared by four experiments. The inner diameters of the flat-mouth needles corresponding to a to d are 0.26 mm, 0.42 mm, 0.52 mm, and 0.61 mm, respectively. The scale in the figure is 2 mm. Figure 2 It can be seen that: as the inner diameter of the needle increases, the size of the macroporous CaAlg gel ball also increases; when the size of the macroporous CaAlg gel ball is small, due to the continuous generation of internal CO2 bubbles, the CaAlg gel formed by cross-linking in the outer layer is squeezed and deformed, thus presenting a non-spherical shape.
[0057] The macroporous CaAlg gel spheres prepared in four groups of experiments were dispersed in deionized water, and their diameters were measured and the coefficient of variation (CV) of the diameters were calculated. When the inner diameters of the needles were 0.26 mm, 0.42 mm, 0.52 mm and 0.61 mm, the diameters of the prepared macroporous CaAlg gel spheres were 1.61 mm, 1.92 mm, 2.08 mm and 2.42 mm, respectively, and the CV values of the diameters were 7.7%, 6.7%, 3.1% and 4.2%, respectively. When the inner diameters of the needles were 0.52 mm and 0.61 mm, the sphericity of the prepared macroporous CaAlg gel spheres was better, and their CV values were relatively lower. Based on this, a needle with an inner diameter of at least 0.42 mm can be selected for preparation, and the specific inner diameter of the needle can be determined according to the actual application requirements. For example, the inner diameter of the needle can usually be selected between 0.5 and 1 mm.
[0058] Example 3
[0059] In this embodiment, millimeter-scale CaAlg gel spheres with an open macroporous structure were prepared using gel precursor solutions with different NaAlg concentrations.
[0060] This embodiment is provided with 4 groups of experiments, and the operation of each group of experiments is basically the same as that of embodiment 1, except that the concentration of NaAlg in the gel precursor solution used in each group of experiments is different. In the gel precursor solution used in the 4 groups of experiments, the concentration of NaHCO3 is 1.5wt%, the concentration of SDS is 0.1wt%, and the concentration of NaAlg is 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt%, respectively.
[0061] The prepared four gel precursor solutions were placed statically for different periods of time to observe how their states changed with the placement time. The results are as follows: Figure 3 As shown. Figure 3It can be seen that: when the concentration of NaAlg in the gel precursor is 0.5wt%, as the standing time increases, the bubbles in the gel precursor quickly dissipate and stratify with the solution, and the gel precursor has obvious stratification when it is standing for less than 5 minutes; when the concentration of NaAlg in the gel precursor is 1wt% and 1.5wt%, the gel precursor begins to stratify after standing for 10min and 20min respectively; when the concentration of NaAlg in the gel precursor is 2wt%, the gel precursor does not stratify after standing for 20min. The increase in the stability of the gel precursor is conducive to the uniform distribution of the number of bubble templates in the gel precursor droplets dripped into the coagulation bath solution, thereby increasing the consistency of the internal pore structure of different gel balls finally prepared.
[0062] The optical photographs of the millimeter-sized CaAlg gel spheres with interconnected macropores (referred to as macroporous CaAlg gel spheres) prepared in the four groups of experiments in this example are shown in FIG. Figure 4 As shown, Figures a to d correspond to the experimental groups with NaAlg concentrations of 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt% in the gel precursor solution, and the scale in the figure is 2mm. Figure 4 It can be seen that when the concentration of NaAlg in the gel precursor is 0.5wt%, the texture of the prepared macroporous CaAlg gel spheres is similar to plastic, and the overall shape is milky white and irregular. This is because when the concentration of NaAlg is low, it is more likely to be oxidized than CaAlg. 2+ The strength of the gel formed after cross-linking is low and it is easily deformed by the squeezing of internal bubbles. When the concentration of NaAlg in the gel precursor solution is 1wt% to 2wt%, the prepared macroporous CaAlg gel spheres are basically white spherical. The prepared macroporous CaAlg gel spheres are dispersed in deionized water, the size of the macroporous CaAlg gel spheres is measured and the CV value of the diameter is calculated. When the concentration of NaAlg in the gel precursor solution is 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt%, the diameters of the prepared macroporous CaAlg gel spheres are 2.15mm, 2.01mm, 2.12mm and 2.08mm respectively, and the CV values of the diameters are 9.7%, 5.4%, 4.4% and 4.4% respectively. With the increase of the concentration of NaAlg in the gel precursor solution, the CV value of the diameter of the macroporous CaAlg gel spheres gradually decreases, and the size distribution becomes more uniform.
[0063] The scanning electron microscopy images of the cross-sections of the macroporous CaAlg gel spheres prepared in the four groups of experiments in this example are as follows: Figure 5 As shown in the figure, a to d correspond to the experimental groups with NaAlg concentrations of 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt% in the gel precursor solution, and the scale bar in the figure is 200μm. Figure 5It can be seen that when the NaAlg concentration in the gel precursor solution is 0.5wt% and 1.0wt%, large-volume pores appear inside the macroporous CaAlg gel spheres, which is caused by the aggregation and coarsening of bubbles. When the NaAlg concentration in the gel precursor solution is 1.5wt% and 2.0wt%, the pores inside the macroporous CaAlg gel spheres are evenly distributed and interconnected.
[0064] The porosity, pore size, and CV values of porosity and pore size of the macroporous CaAlg gel balls prepared by the four groups of experiments of the present embodiment are calculated. When the concentration of NaAlg in the gel precursor solution is 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt%, the porosity of the macroporous CaAlg gel balls is 77.54%, 67.21%, 63.11% and 61.08% respectively, the CV values of porosity are 10.8%, 5.1%, 2.7% and 2.4% respectively, the average pore size of the macroporous CaAlg gel balls is 240.64μm, 162.27μm, 143.67μm and 128.34μm respectively, and the CV values of pore size are 14.3%, 19.6%, 21.7% and 17.5% respectively. The higher the concentration of NaAlg in the gel precursor solution, the smaller the difference in the porosity of the macroporous CaAlg gel balls. The CV values of the pore sizes of the macroporous CaAlg gel spheres prepared in the four groups of experiments were distributed between 10% and 20%, which indicates that the pore sizes inside the macroporous CaAlg gel spheres are mixed, not a single large or small pore size, which is beneficial to cell growth and differentiation.
[0065] From the above content, it can be seen that considering the morphology and pore structure of the gel spheres and other factors, the concentration of NaAlg in the gel precursor solution is preferably 1.5 wt % to 2 wt %.
[0066] Example 4
[0067] In this embodiment, millimeter-scale CaAlg gel spheres with an open macroporous structure were prepared using gel precursor solutions with different NaHCO3 concentrations.
[0068] This embodiment has 4 groups of experiments, and the operation of each group of experiments is basically the same as that of Example 1, except that the concentration of NaHCO3 in the gel precursor solution used in each group of experiments is different. In the gel precursor solution used in the 4 groups of experiments, the concentration of NaAlg is 1.5wt%, the concentration of SDS is 0.1wt%, and the concentration of NaHCO3 is 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt%, respectively.
[0069] The optical photographs of the millimeter-sized CaAlg gel spheres with interconnected macropores (referred to as macroporous CaAlg gel spheres) prepared in the four groups of experiments in this example are shown in FIG. Figure 6As shown, the a-d figures correspond to the experimental groups of NaHCO3 concentration of 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt% in the gel precursor solution, and the scale in the figure is 2mm. The prepared macroporous CaAlg gel balls are dispersed in deionized water, the diameter of the macroporous CaAlg gel balls is measured and the CV value of the diameter is calculated. When the NaHCO3 concentration in the gel precursor solution is 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt%, the diameter of the prepared macroporous CaAlg gel balls is 1.81mm, 2.19mm, 2.12mm and 2.29mm respectively, and the CV value of the diameter is 3.0%, 3.5%, 4.2% and 4.3% respectively. With the increase of NaHCO3 concentration, the overall size of the macroporous CaAlg gel balls gradually increases and the surface gradually becomes uneven, with many protrusions added, which is because the amount of bubbles generated gradually increases, and the outer layer cross-linked CaAlg is squeezed and caused.
[0070] The scanning electron microscopy images of the cross-sections of the macroporous CaAlg gel spheres prepared in the four groups of experiments in this example are as follows: Figure 7 As shown, Figures a to d correspond to the experimental groups with NaHCO3 concentrations of 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt% in the gel precursor solution, and the scale bar in the figure is 200μm. Figure 7 It can be seen that the pores inside the macroporous CaAlg gel are all through holes, which are beneficial to enhancing the connection between the loaded cells and improving the functional expression ability of the cells. With the increase of NaHCO3 concentration, the pore density inside the macroporous CaAlg gel ball increases.
[0071] The porosity, pore size, and CV values of the porosity and pore size of the macroporous CaAlg gel spheres prepared in the four groups of experiments in this embodiment were calculated. When the concentration of NaHCO3 in the gel precursor solution was 0.5wt%, 1.0wt%, 1.5wt% and 2.0wt%, the porosity of the macroporous CaAlg gel spheres was 49.40%, 54.69%, 63.11% and 67.89%, respectively. The porosity increased with the increase of NaHCO3 concentration. It can be seen that increasing the NaHCO3 concentration can provide more room for the generation of CO2 bubbles. There are more nucleation sites, and the CV values of porosity are 2.6%, 3.5%, 2.7% and 5.5%, respectively, indicating that the pore structure inside the macroporous CaAlg gel sphere is relatively uniform; the average pore sizes of the macroporous CaAlg gel spheres are 144.19μm, 133.22μm, 143.66μm and 142.65μm, respectively, and the CV values of the pore size are 12.0%, 13.4%, 21.2% and 21.2%, respectively. The gradual increase in the CV value of the pore size indicates that increasing the NaHCO3 concentration will increase the disorder of bubble growth.
[0072] Example 5
[0073] In this embodiment, etchants of different types and concentrations are used to etch the macroporous CaAlg gel spheres.
[0074] (1) The operation is the same as step (1) of Example 1.
[0075] (2) The same operation as step (2) of Example 1 was performed to prepare millimeter-sized CaAlg gel spheres with interconnected macropores inside (referred to as macroporous CaAlg gel spheres).
[0076] (3) Add the macroporous CaAlg gel spheres to the etchant aqueous solution at a ratio of 4 g of macroporous CaAlg gel spheres to 1 L of etchant aqueous solution, and etch for 120 min at a stirring speed of 20 rpm. After the etching is completed, the etchant aqueous solution is immediately sucked away and a large amount of deionized water is added to terminate the reaction, and the solid-liquid separation is performed. The obtained gel spheres are washed with deionized water for 2 to 3 times to obtain open-pore CaAlg gel spheres. During the etching process, photos are taken at intervals to record the surface morphology changes of the macroporous CaAlg gel spheres.
[0077] The concentrations of the etchants used and their aqueous solutions are: sodium citrate (33.50 g / L), sodium bicarbonate (9.57 g / L), sodium acetate (9.35 g / L), sodium chloride (6.66 g / L), sodium hydroxide (4.56 g / L), potassium citrate (36.96 g / L), ammonium citrate (27.71 g / L), and ferric citrate (27.90 g / L).
[0078] Figure 8 This is an optical photograph of a macroporous CaAlg gel ball during etching. The scale in the figure is 1 mm. Figure 8 It can be seen that sodium bicarbonate, sodium acetate and sodium chloride have no chemical effect on the macroporous CaAlg gel spheres; the macroporous CaAlg gel spheres gradually begin to dissolve and release some encapsulated bubbles after being immersed in the sodium hydroxide aqueous solution for 60 minutes, and most of the macroporous CaAlg gel spheres are etched after being immersed for 120 minutes; the ferric citrate aqueous solution has a certain swelling effect on the macroporous CaAlg gel spheres, but no obvious etching occurs; the sodium citrate, potassium citrate and ammonium citrate aqueous solutions have an etching effect on the macroporous CaAlg gel spheres, but the etching rates are different, with ammonium citrate being the fastest, followed by sodium citrate, and potassium citrate being the slowest.
[0079] (4) Adjust the concentration of the etchant aqueous solution in step (3) and repeat the operation of step (3). The concentration of the etchant aqueous solution used is: sodium citrate (6.7 g / L), sodium bicarbonate (9.57 g / L), sodium acetate (9.35 g / L), sodium chloride (6.66 g / L), sodium hydroxide (4.56 g / L), potassium citrate (7.39 g / L), ammonium citrate (5.54 g / L), and ferric citrate (27.90 g / L).
[0080] The open-pore CaAlg gel spheres obtained by etching for different times were tested by scanning electron microscopy. Fig. 9 As shown, Fig. 9 In the a~h diagrams of , the corresponding etchants are sodium citrate, sodium bicarbonate, sodium acetate, sodium chloride, sodium hydroxide, potassium citrate, ammonium citrate and ferric citrate, and the corresponding etching times are 20min, 120min, 120min, 120min, 120min, 40min, 20min and 120min, respectively; the scale in the diagram is 1mm. Fig. 9 It can be seen that sodium bicarbonate, sodium acetate and sodium chloride have basically no etching effect on macroporous CaAlg gel spheres; ferric citrate has weak etching effect on macroporous CaAlg gel spheres, and uneven etching occurs after immersion for 120 minutes; macroporous CaAlg gel spheres are etched after immersion in sodium citrate and ammonium citrate aqueous solutions for 20 minutes, among which the etching of sodium citrate is more uniform; macroporous CaAlg gel spheres are etched after immersion in potassium citrate aqueous solution for 40 minutes, and many holes can be observed on their surface. In general, the etching effect of sodium citrate and potassium citrate is relatively better.
[0081] (5) Using potassium citrate as an etchant, repeat the operation of step (3). A total of 3 groups of experiments were set up, as follows:
[0082] Experimental group ①, the potassium citrate concentrations were 30g / L, 35g / L, 40g / L, 45g / L and 50g / L, respectively, and the etching time was 5min. The SEM images of the prepared open-pore CaAlg gel spheres are shown in Fig.10 As shown in Figures a1 to a5;
[0083] Experimental group ②, the potassium citrate concentrations were 0.2g / L, 0.4g / L, 0.6g / L, 0.8g / L and 1.0g / L, respectively, and the immersion time was 120min. The scanning electron microscopy images of the prepared open-pore CaAlg gel spheres are shown in Fig.10 As shown in Figures b1 to b5;
[0084] Experimental group ③, the potassium citrate concentrations were 5g / L, 10g / L, 15g / L, 20g / L and 25g / L, and the immersion time was 120min. The scanning electron microscopy images of the prepared open-pore CaAlg gel spheres are shown in Fig.10 As shown in the figure c1~c5.
[0085] Depend on Fig.10 It can be seen that in experimental group ①, under the conditions of high concentration and short etching time, the surface of the prepared open-pore CaAlg gel sphere was covered with open pores, but the structure of the open-pore CaAlg gel sphere collapsed, which was mainly caused by the high concentration of the etchant. In experimental group ②, under the conditions of low concentration and long etching time, the surface of the prepared open-pore CaAlg gel sphere did not show a large area of open pore structure, and wrinkling occurred. This is because the etching time is too long, and the etchant gradually diffuses into the interior of the gel sphere and dissolves the gel with a low degree of internal cross-linking. In experimental group ③, when the concentration of potassium citrate is 10-15g / L, the surface of the open-pore CaAlg gel sphere prepared by etching for 5min has a relatively uniform distribution of open macropores, and the sphere does not collapse.
[0086] In this step, the porosity of the open pores on the surface of the open-pored CaAlg gel balls prepared at potassium citrate concentrations of 10 g / L and 15 g / L was 26.41% and 37.73%, respectively, and the average pore size of the open pores on the surface of the open-pored CaAlg gel balls was 159.50 μm and 194.37 μm, respectively.
[0087] Example 6
[0088] In this example, the ability of the millimeter-sized CaAlg gel spheres with an open macroporous structure prepared in Example 1 (referred to as open-pore CaAlg gel spheres) to adsorb cells was tested.
[0089] HepG2 cells in the logarithmic growth phase were digested with trypsin to prepare a single cell suspension with a cell density of 5×10 6 / mL. Soak the gel balls in PBS buffer to fully swell, and sterilize with ultraviolet light. After sterilization, discard the PBS buffer and soak the gel balls with complete culture medium. Spread the gel balls soaked in complete culture medium on a 35mm culture dish, add 1.5mL of cell suspension, and after observing that the cells are absorbed into the gel balls, transfer the cell-loaded gel balls to a new culture dish, add 4% paraformaldehyde solution, fix at room temperature for 20 minutes, discard the paraformaldehyde solution, and wash with PBS buffer to remove the residual paraformaldehyde solution. Then use 10μg·mL -1The cells were stained with 4',6-diamidino-2-phenylindole (DAPI) solution at room temperature in the dark for 5 min, and the cells were washed with PBS buffer and observed under a fluorescence microscope. The open-pore CaAlg gel spheres and macroporous CaAlg gel spheres prepared in Example 1 were used as the experimental group and the control group, respectively.
[0090] The adsorption capacity of gel balls to cells and the distribution of cells in gel balls are crucial for cell culture. It is necessary that cells can be adsorbed into the gel balls and dispersed as evenly as possible. After the gel balls adsorb the cell suspension for 30 minutes, transfer it to a new culture dish and stain the cells with DAPI solution. Blue fluorescence can be observed under a fluorescence microscope, such as Fig.11 As shown, a and b are fluorescence images of macroporous CaAlg gel spheres after adsorption of HepG2 cells, and c and d are fluorescence images of open-pore CaAlg gel spheres after adsorption of HepG2 cells. a and c are bright fields, b and d are fluorescence fields, and the scale bar in the figure is 500 μm. Fig.11 It can be seen that the open-pore CaAlg gel sphere is extremely transparent after being soaked in PBS buffer, and the complex pores inside can be vaguely seen under the bright field; the blue fluorescence representing cells is almost invisible in the macroporous CaAlg gel sphere, and many HepG2 cells are adsorbed inside the open-pore CaAlg gel sphere, and are evenly dispersed in the pores inside the gel sphere. It can be seen that the present invention effectively improves the ability of the gel sphere to adsorb cells after etching to form open and connected macropores.
[0091] Example 7
[0092] In this example, the activity and proliferation of HepG2 cells in the millimeter-sized CaAlg gel spheres with an open macroporous structure prepared in Example 1 (referred to as open-pore CaAlg gel spheres) were tested.
[0093] (1)① HepG2 cells in the logarithmic growth phase were digested with trypsin to prepare a single cell suspension with a cell density of 5×10 6 After sterilizing, the gel balls (the macroporous CaAlg gel balls and the open-pore CaAlg gel balls prepared in Example 1) were immersed in a complete culture medium solution, and the gel balls were pre-covered in a 35 mm culture dish, and then 1.5 mL of the cell suspension was added. After observing that the cells were absorbed into the gel balls, the cell-loaded gel balls were transferred to a new culture dish, and 1 mL of fresh complete culture medium was added, and the cells were cultured in a 5% CO2 and 37°C constant temperature cell culture incubator.
[0094] ② After culturing for 24h, 48h and 72h, discard the original culture medium, wash 2-3 times with PBS buffer, add 1mL of cell double staining working solution (Calcein-AM: 2μM, PI: 4.5μM), and stain for 15min at room temperature in the dark.
[0095] ③After staining, discard the staining solution and wash with PBS buffer, and observe the cell survival under a fluorescence microscope. The results are as follows Fig.12 shown.
[0096] Depend on Fig.12 It can be seen that neither green fluorescence representing live cells nor red fluorescence representing dead cells was observed on the macroporous CaAlg gel spheres, which indicates that it is difficult for macroporous CaAlg gel spheres to adsorb HepG2 cells from the beginning. The HepG2 cells in the perforated CaAlg gel spheres showed strong green fluorescence after culturing for 24h, 48h and 72h. After culturing for 48h and 72h, a small number of dead cells appeared inside the gel spheres. As the culture time increased, the number of live cells gradually increased, and the cell morphology gradually agglomerated, which was completely inconsistent with the morphology during 2D adherent culture. It is shown that the perforated CaAlg gel spheres provided by the present invention are suitable as carriers for in vitro 3D cell culture.
[0097] (2)① HepG2 cells in the logarithmic growth phase were digested with trypsin to prepare a single cell suspension with a cell density of 5×10 6 After sterilizing, the gel balls (the macroporous CaAlg gel balls and the open-pore CaAlg gel balls prepared in Example 1) were immersed in a complete culture medium solution, and the gel balls were pre-covered in a 35 mm culture dish, and then 1.5 mL of the cell suspension was added. After observing that the cells were absorbed into the gel balls, the cell-loaded gel balls were transferred to a new culture dish, and 1 mL of fresh complete culture medium was added, and the cells were cultured in a 5% CO2 and 37°C constant temperature cell culture incubator.
[0098] ② After culturing for 24h, 48h and 72h, discard the original culture medium, add 1mL of complete culture medium containing 10% CCK-8 solution (experimental group), and incubate at 37℃ for 2h. Set up complete culture medium containing 10% CCK-8 solution as the control group and incubate at 37℃ for 2h together with the experimental group.
[0099] ③After incubation, collect the supernatant in the culture dish into a 96-well plate and measure the OD value at 450nm using an enzyme marker. Set up six parallel experiments for each group, and finally take the average value of the OD value of each group as the six parallel experiments.
[0100] After culturing cells with open-pore CaAlg gel spheres for 24h, 48h, and 72h, the activity of HepG2 cells was above 95%. Fig.13Figure a shows that the open-pore CaAlg gel spheres are suitable as carriers for cell culture. The cell proliferation of HepG2 cells after culturing with macroporous CaAlg gel spheres and open-pore CaAlg gel spheres for 24h, 48h and 72h is shown in Figure a. Fig.13 As shown in Figure b. After the open-pore CaAlg gel spheres were used to culture HepG2 cells for 48h and 72h, the OD values were 1.4 times and 2.3 times that of the 24h culture, while the OD values did not change substantially after the macroporous CaAlg gel spheres were used to culture HepG2 cells for 24, 48h and 72h, indicating that the open-pore CaAlg gel spheres of the present invention can maintain the conditions for cell growth and proliferation and ensure the diffusion supply of cell nutrients.
[0101] Example 8
[0102] In this example, a specific secretion experiment of HepG2 cells in the millimeter-sized CaAlg gel spheres with open macroporous structure (hereinafter referred to as open-pore CaAlg gel spheres) prepared in Example 1 was conducted. The macroporous CaAlg gel spheres prepared in step (2) of Example 1 were used as a control group, and the open-pore CaAlg gel spheres prepared in step (3) of Example 1 were used as an experimental group to study the secretion concentrations of the two at different culture times after cell adsorption.
[0103] (1) Detection of urea concentration secreted by cells using double antibody sandwich ELISA
[0104] HepG2 cells in the logarithmic growth phase were digested with trypsin to prepare a single cell suspension with a cell density of 5×10 6 / mL. After sterilizing the gel balls, soak them in a complete culture medium solution. Pre-spread the gel balls in a 35mm culture dish, then add 1.5mL of cell suspension. After observing that the gel balls are absorbed into the cells, transfer the gel balls loaded with cells to a new 35mm culture dish to culture the cells, and place them in a constant temperature cell culture incubator with 5% CO2 and 37°C. After culturing for 24h, 48h and 72h, transfer them to a sterile centrifuge tube, centrifuge at 2000rpm for 20min, and collect the supernatant. Add 50μL of urea standard and the collected supernatant to the pre-coated well plate, then add 100μL of HPR-labeled detection antibody, seal the plate and incubate at room temperature for 60min. After tapping and washing the plate 5 times, add 50μL of color developer A and color developer B in turn, seal the plate, and incubate at 37°C in the dark for 15min. Finally, add 50μL of acidic solution to terminate the reaction, and measure the absorbance value at a wavelength of 450nm with an enzyme reader within 15min. Four parallel experiments were set up, and the absorbance value of each group was finally taken as the average value of the four parallel experiments.
[0105] Fig.14Figures a and b show the OD value and urea concentration of urea in the supernatant after HepG2 cells were cultured for different time periods using macroporous CaAlg gel spheres and open-pore CaAlg gel spheres, respectively. The urea concentration in the supernatant showed a negative correlation with the increase in culture time, which may be due to the rapid degradation of urea or the complexity of maintaining and expressing the functions of hepatocytes themselves.
[0106] (2) Detection of cytochrome P450 (CYP450) concentration in cells using competitive ELISA
[0107] HepG2 cells in the logarithmic growth phase were digested with trypsin to prepare a single cell suspension with a cell density of 5×10 6 / mL. After sterilizing the gel balls, soak them in a complete culture medium solution. Pre-cover the 35mm culture dish with gel balls, then add 1.5mL of cell suspension. After observing that the gel balls are absorbed by the cells, transfer the gel balls loaded with cells to a new 35mm culture dish to culture the cells, and culture them in a constant temperature cell culture incubator with 5% CO2 and 37°C. After culturing for 24h, 48h and 72h, discard the original culture medium, add PBS buffer containing 5mol / L citric acid, transfer the mixture to a sterile centrifuge tube after dissolving overnight, centrifuge at 2000rpm for 20min, and discard the supernatant. Add 100μL of cell lysis solution to the precipitate, react at 4°C for 30min, centrifuge at 2000rpm for 20min, and collect the supernatant. Add 50μL CYP450 standard and collected supernatant to the pre-coated well plate, then add 50μL biotinylated antigen working solution to seal the plate and incubate at 37℃ for 30min. After tapping and washing the plate 5 times, add 50μL avidin-HPR working solution, seal the plate and incubate at 37℃ for 30min. Then tap and wash the plate 5 times, add 50μL A colorimetric agent and 50μL B colorimetric agent in sequence, seal the plate, and react at 37℃ in the dark for 10min. Finally, add 50μL acidic solution to terminate the reaction, and measure the absorbance value at 450nm wavelength with an enzyme reader within 10min. Set up four parallel experiments, and finally take the average value of the absorbance value of each group as the average of the four parallel experiments.
[0108] Fig.15 Figures a and b show the OD value and CYP450 concentration of the supernatant after HepG2 cells were cultured for different time periods using macroporous CaAlg gel spheres and open-pore CaAlg gel spheres, respectively. The concentration of CYP450 in macroporous CaAlg gel spheres was always lower than the lowest concentration of the CYP450 standard, and its specific concentration could not be calculated using the fitting curve. Fig.15In Figure b, NA is used to represent the concentration of CYP450 in the open-pore CaAlg gel spheres. The concentration of CYP450 in the open-pore CaAlg gel spheres gradually increased with the culture time, indicating that the functional expression of HepG2 cells was maintained. The above experimental results show that the physiological function of HepG2 cells is improved in the open-pore CaAlg gel spheres, and the open-pore CaAlg gel spheres are suitable as carrier scaffolds for cell culture.
Claims
1. Millimeter-sized calcium alginate gel spheres with open macroporous structure, It is characterized in that The matrix material of the gel ball is calcium alginate. The interior of the gel ball has a mutually interpenetrating micron-scale pore structure, and the mutually interpenetrating micron-scale pore structure inside the gel ball is opened on the surface of the gel ball. The average pore size of the micron-scale pore structure inside the gel ball is 120 to 160 μm. The particle size of the gel ball when it reaches swelling equilibrium in water is 2 to 5 mm.
2. The millimeter-sized calcium alginate gel sphere with an open macroporous structure according to claim 1, It is characterized in that The average pore size of the pore structure on the surface of the gel ball is 150-200 μm.
3. The millimeter-sized calcium alginate gel sphere with an open macroporous structure according to claim 2, It is characterized in that The porosity of the pore structure on the surface of the gel ball is 20% to 40%.
4. The millimeter-sized calcium alginate gel sphere with an open macroporous structure according to any one of claims 1 to 3, It is characterized in that The porosity of the pore structure inside the gel ball is 50% to 70%.
5. A method for preparing the millimeter-sized calcium alginate gel spheres with an open macroporous structure according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) dissolving sodium alginate, a porogen and a water-soluble anionic surfactant in water, homogenizing and emulsifying the resulting mixed solution to incorporate bubbles into the mixed solution, and obtaining a gel precursor solution; in the gel precursor solution, the concentration of sodium alginate is 1.5wt% to 2wt%, the concentration of the porogen is 1wt% to 2wt%, and the concentration of the water-soluble anionic surfactant is 0.05wt% to 0.15wt%; the porogen is sodium bicarbonate or potassium bicarbonate; Dissolving a water-soluble calcium salt and glacial acetic acid in water to obtain a coagulation bath solution, wherein the concentration of the water-soluble calcium salt in the coagulation bath solution is 5wt% to 15wt%, and the concentration of the glacial acetic acid is 5wt% to 15wt%; (2) dripping the gel precursor into the coagulation bath solution through an injection needle, the sodium alginate in the gel precursor droplets dripping into the coagulation bath solution undergoes a cross-linking reaction with the calcium ions, and at the same time, the porogen in the gel precursor droplets dripping into the coagulation bath solution reacts with glacial acetic acid to generate CO in the gel precursor droplets. 2 The gas causes the bubbles in the gel precursor droplets to be connected, and after the gel precursor droplets are cross-linked and solidified, the solid-liquid separation is performed, and the unreacted water-soluble calcium salt and glacial acetic acid in the obtained solid phase are removed by washing, and freeze-dried to obtain millimeter-sized calcium alginate gel spheres with interconnected macropores inside; (3) immersing the gel sphere obtained in step (2) in an etchant aqueous solution, etching under stirring, so that the etchant is complexed with calcium ions in the calcium alginate on the surface of the gel sphere to form an open-pore structure on the surface of the gel sphere, immediately replacing the etchant aqueous solution with water to terminate the reaction between the etchant and the calcium ions, separating the solid and the liquid, washing and drying the obtained solid phase, and obtaining millimeter-sized calcium alginate gel spheres with an open macroporous structure; the etchant is potassium citrate or sodium citrate, and the concentration of the etchant aqueous solution is 10-15 g / L.
6. The method for preparing the millimeter-sized calcium alginate gel spheres with an open macroporous structure according to claim 5, It is characterized in that In step (3), the etching time is controlled to be 3 to 10 minutes.
7. The method for preparing the millimeter-sized calcium alginate gel spheres with an open macroporous structure according to claim 5, It is characterized in that In step (2), the gel precursor solution is dripped into the coagulation bath solution through an injection needle with an inner diameter of 0.5 to 1 mm.
8. A method for preparing the millimeter-sized calcium alginate gel spheres with an open macroporous structure according to any one of claims 5 to 7, It is characterized in that In step (2), the gel precursor solution is dripped into the coagulation bath solution through the injection needle by the injection pump at a flow rate of 15 to 25 mL / h.
9. A method for preparing the millimeter-sized calcium alginate gel spheres having an open macroporous structure according to any one of claims 5 to 7, It is characterized in that In step (2), the cross-linking time is controlled to be 10 to 15 hours.
Citation Information
Patent Citations
Preparation method of macroporous cross-linked sodium alginate gel beads
CN102226012A
Spherical calcium alginate gel micro-particle preparation method
CN104829850A
Preparation method for oil-water separation type alginate aerogel having nano-micron gradient hierarchical pore structure
CN110698722A
Preparation method of interpenetrating polymer network (IPN)scaffold for cell delivery comprising sodium hyaluronate and sodium alginate
KR1020120086948A
Self-adhesive hemostatic repair gel with multi-scale pore network, and preparation method therefor and use thereof
WO2024087678A1