Organic polymer reinforced natural rubber compound material and preparation method thereof
By using specific organic polymer reinforcement particles and modifiers in rubber materials, the high heat generation problem of rubber materials under high speed driving and rugged road usage conditions is solved, achieving both high load bearing and low heat generation, and improving Comprehensive properties of materials.
Patent Information
- Application Number
- CN202411337179.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-29
AI Technical Summary
In the high-speed driving and rugged road conditions, existing rubber materials are difficult to meet the comprehensive performance requirements such as high load bearing, low heat generation, and tear resistance. The reinforcement of carbon black filler leads to excessive heat generation, and the dispersion of new fillers is poor, which affects the impact of Material properties.
Use organic polymer reinforced particles that maintain a specific aggregated structure below 80°C to replace part of carbon black, combine dihydrazine natural rubber modifiers and tetrazine organic polymer modifiers to enhance the dispersion effect of carbon black filler. Reduce heat generation of materials and maintain high load-bearing properties.
It effectively reduces the heat generation of rubber mixed rubber materials, improves high-temperature mechanical properties and load-bearing capacity, and optimizes the comprehensive performance of the materials, which is suitable for use needs under severe working conditions.
Smart Images

Figure BDA0005058576720000071 
Figure BDA0005058576720000081 
Figure BDA0005058576720000082
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber materials, and in particular relates to an organic polymer reinforced natural rubber compound material and a preparation method thereof. Background Art
[0002] Rubber materials are widely used in tires, tracks and other fields. Due to the characteristics of their use conditions, the materials have performance requirements such as high load-bearing, low heat generation, and tear resistance. The comprehensive performance of current rubber materials under use conditions such as high-speed driving and rough roads still cannot meet the use requirements, which seriously affects their reliability. Natural rubber has excellent comprehensive properties due to its unique strain-induced crystallization mechanism and is a widely used rubber material. Unfilled natural rubber materials have low strength and hardness and cannot meet the requirements of high load-bearing, so they must be reinforced with fillers such as carbon black. After adding carbon black, due to the friction between the carbon black filler itself and the natural rubber molecular chain, the material will generate too much heat during use, which will lead to material failure and affect the service life and safety.
[0003] Reducing the amount of carbon black can significantly reduce the heat generation of natural rubber compound materials, but its mechanical properties such as strength and hardness will also decrease, and the material's load-bearing capacity is obviously insufficient. At present, the common practice is to use new fillers (carbon nanotubes, graphene, short fibers, etc.) to replace part of the carbon black to achieve a balance between load-bearing capacity and heat generation. However, this type of new filler has low surface activity and is not easy to disperse in the natural rubber matrix. It may even agglomerate, which leads to the degradation of material properties. Although the dispersion problem of such fillers can be improved to a certain extent by surface treatment and other methods, the complexity of the process and the resulting cost issues also affect the practical application of the material.
[0004] Therefore, how to reduce the amount of carbon black without causing a decrease in other properties through material design, and then achieve overall optimization of properties such as high load-bearing capacity, low heat generation, and high temperature resistance in natural rubber compound materials, is of great significance for meeting the use requirements under harsh working conditions. Summary of the invention
[0005] In view of the shortcomings and defects of the prior art, the present invention provides an organic polymer reinforced natural rubber mixed with natural rubber compound material and a preparation method thereof.
[0006] The object of the present invention is achieved by selecting a material that can maintain a specific aggregate structure (crystallization, phase separation, etc.) at a temperature not exceeding 80°C as an organic polymer reinforcing particle, using its microphase structure to reinforce the natural rubber matrix, and replacing the filling amount of carbon black reinforcing filler in proportion, thereby reducing the friction between the filler itself and the rubber molecular chain during the use of the product, thereby reducing the heat generation. At the same time, the reinforcing effect of the organic polymer reinforcing particles can also make up for the performance problems that may be caused by the reduction in the amount of reinforcing filler, so that it can continue to maintain the function of high load-bearing at room temperature and high temperature. The dihydrazide natural rubber modifier used can utilize the activity of the hydrazide group to react with active groups such as aldehyde groups on the natural rubber chain. The tetrazine organic polymer modifier used can utilize the activity of the tetrazine group to react with the carbon-carbon double bonds on the organic polymer reinforcing particles. The polar groups on the above modifiers can also interact with the polar groups on the surface of the carbon black filler to enhance the interfacial bonding strength between the natural rubber matrix and the organic polymer reinforcing particles and the carbon black reinforcing filler, further optimize the dispersion effect of the carbon black reinforcing filler, and achieve an improvement in the overall performance of the material.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0008] An organic polymer reinforced natural rubber compound material, comprising:
[0009] Natural rubber 100 parts by weight
[0010] Natural rubber modifier 0.2-1.0 parts by weight
[0011] 5-15 parts by weight of organic polymer reinforcement particles
[0012] 0.5-1.5 parts by weight of organic polymer modifier
[0013] Carbon black reinforcing filler 45-55 parts by weight
[0014] 8-20 parts by weight of auxiliary agent
[0015] The organic polymer reinforcement particles are syndiotactic 1,2-polybutadiene (s-PB) materials with high rigidity crystalline structure;
[0016] The melting point range of the s-PB material is 95-126°C;
[0017] The total amount of the organic polymer reinforcing particles and the carbon black reinforcing filler is 50 to 60 parts by weight;
[0018] The natural rubber is one of smoked sheet rubber and full latex standard rubber;
[0019] The natural rubber modifier is a dihydrazide compound, preferably terephthaloyl dihydrazide or sebacic acid dihydrazide;
[0020] The organic polymer modifier is a tetrazine compound, preferably 3-methyl-6-(2-pyridyl)-1,2,4,5-tetrazine or 3,6-bis(4-hydroxyphenyl)-1,2,4,5-tetrazine;
[0021] The auxiliary agent includes 3-5 parts of zinc oxide, 2-3 parts of stearic acid, 1-3 parts of antioxidant, 0.5-2 parts of coupling agent, 1-4 parts of sulfur, and 0.5-3 parts of accelerator;
[0022] The carbon black reinforcing filler is one of carbon black N220, carbon black N330, and carbon black N550; the antioxidant is one of antioxidant 4010NA, antioxidant 4020, and antioxidant RD; the accelerator is one of accelerator NS, accelerator CZ, and accelerator DM; and the coupling agent is silane coupling agent Si-69.
[0023] The present invention relates to an organic polymer reinforced natural rubber compound material, and the preparation method thereof comprises the following steps:
[0024] 1) One-stage mixing: natural rubber and dihydrazide compounds are put into an internal mixer and mixed at a speed of 30-45 rpm for 90-100 seconds, organic polymer modifiers and tetrazine modifiers are put into the internal mixer and mixed for 100-120 seconds, zinc oxide, stearic acid, antioxidant, coupling agent and carbon black reinforcing filler are added to the internal mixer, and the mass is lifted and pressed every 30-40 seconds. When the temperature of the rubber material reaches 125-130°C, the rubber material is continuously mixed for 80-95 seconds and then discharged.
[0025] 2) Second stage mixing: the first stage mixed rubber of step 2) is put into an internal mixer together with sulfur and an accelerator, and mixed at a speed of 20-30 rpm. When the temperature of the rubber material reaches 100-115° C., the rubber material is discharged and placed to cool, thereby obtaining a natural rubber mixed rubber material.
[0026] Beneficial effects of the present invention:
[0027] Compared with the prior art, the present invention uses organic polymer reinforcing particles and carbon black reinforcing fillers together, effectively improving the problem of excessive heat generation of natural rubber compound materials caused by a large number of carbon black reinforcing fillers, while allowing the natural rubber compound materials to continue to maintain a high load-bearing capacity; at the same time, the reasonable content of organic polymer reinforcing particles when the two are used together is proposed, and the content directly affects the performance of the natural rubber compound material. When the proportion of organic polymer reinforcing particles is too high, the strength and other properties of the material will deteriorate, and when the proportion of organic polymer reinforcing particles is too low, the heat generation of the material is not significantly reduced.
[0028] At the same time, the present invention adopts natural rubber modifier and organic polymer modifier to modify the molecular chains of natural rubber and organic polymer reinforcing particles, thereby enhancing the interface interaction between them and carbon black reinforcing fillers, further improving the dispersion effect of carbon black reinforcing fillers, improving the tensile strength and high-temperature mechanical properties of the material, and reducing heat generation.
[0029] The multi-stage feeding preparation method adopted by the present invention first mixes the natural rubber with the corresponding modifier, then adds the organic polymer reinforcement particles and the modifier, and specifies the mixing temperature and time before rubber discharge, which ensures that the modifier can fully react and avoids excessive mixing of the rubber.
[0030] In order to better illustrate the technical effect of the present invention, the natural rubber compound material obtained by the formula and preparation method of the present invention was vulcanized in a flat vulcanizer at 145°C for 20 min to prepare a vulcanized rubber sample, and the performance of the vulcanized rubber sample was tested according to the following test standards:
[0031] Mechanical properties: The tensile properties of the vulcanized rubber are tested according to GB / T 528-2009, including 100% tensile stress, tensile strength and elongation at break;
[0032] Shore A hardness: Test the hardness of vulcanized rubber according to GB / T 531.1-2008;
[0033] Compression fatigue heat generation: Test the compression fatigue heat generation performance of vulcanized rubber in accordance with GB / T 1687.3-2016;
[0034] High temperature mechanical properties: The temperature is adjusted according to GB / T 2941-2006. The high temperature tensile strength of the vulcanized rubber is tested according to GB / T 528-2009. The test temperature is 80±1℃.
[0035] The test results show that the compression fatigue heat generation of the mixed rubber material prepared by the formula and preparation method provided by the present invention is significantly reduced to 15.9°C, the high-temperature tensile strength is increased to 13.9MPa, and the original hardness, tensile strength and other load-bearing properties can be basically maintained, with excellent comprehensive performance. The present invention is suitable for fields such as wheeled vehicle tire tread rubber and tracked vehicle road wheel hanging rubber that require rubber materials to have both high load-bearing and low heat generation performance. DETAILED DESCRIPTION
[0036] The present invention is further described below in conjunction with specific embodiments, but is not intended to limit the scope of the present invention.
[0037] In order to more clearly describe the beneficial effects achieved by the scheme of the present invention, on the basis of the preparation method of the present invention, a rubber compound material was prepared by adding different amounts of organic polymer reinforcing particles, carbon black reinforcing fillers, natural rubber modifiers, organic polymer modifiers, etc., and its performance was investigated and compared with the scheme of the present invention, see Comparative Examples 1-9 for details, and the test results are shown in Table 2.
[0038] Example 1
[0039] An organic polymer reinforced natural rubber compound material comprises the following components by weight: 100 parts of natural rubber (commercially available Indonesian No. 1 smoked rubber), 0.5 parts of terephthaloyl hydrazide, 5 parts of syndiotactic 1,2-polybutadiene material (s-PB, JSRRB840, melting point 126°C), 1 part of 3-methyl-6-(2-pyridyl)-1,2,4,5-tetrazine, 55 parts of carbon black N220, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 0.5 parts of coupling agent si-69, 2.5 parts of sulfur and 1 part of accelerator CZ. The formula is shown in Table 1.
[0040] Natural rubber and terephthalic acid hydrazide are put into an internal mixer and mixed at a speed of 40 rpm for 90 seconds. Organic polymer modifiers and tetrazine modifiers are put into the internal mixer and mixed for 120 seconds. Zinc oxide, stearic acid, antioxidant, coupling agent and carbon black reinforcing filler are added to the internal mixer. The mass is lifted and pressed every 30 seconds. When the temperature of the rubber material reaches 130°C, the mass is mixed for 90 seconds to discharge the rubber to obtain a mixed rubber.
[0041] A section of mixed rubber, sulfur and an accelerator are put into an internal mixer and mixed at a speed of 25 rpm. When the temperature of the rubber material reaches 110° C., the rubber is discharged and sliced, and the natural rubber mixed rubber material is obtained after being left to cool.
[0042] The performance test results are shown in Table 2.
[0043] Example 2
[0044] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, s-PB (JSR RB840, melting point 126°C) 10 parts, carbon black N220 50 parts, the other components are the same, the formula is shown in Table 1, and the performance test results are shown in Table 2.
[0045] Example 3
[0046] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, s-PB (JSR RB840, melting point 126°C) 15 parts, carbon black N220 45 parts, the other components are the same, the formula is shown in Table 1, and the performance test results are shown in Table 2.
[0047] Example 4
[0048] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, s-PB (JSR RB840, melting point 126°C) 5 parts, carbon black N220 50 parts, the other components are the same, the formula is shown in Table 1, and the performance test results are shown in Table 2.
[0049] Example 5
[0050] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material contains 45 parts of carbon black N220 by weight, and the other components are the same. The formula is shown in Table 1, and the performance test results are shown in Table 2.
[0051] Example 6
[0052] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material contains 0.2 parts of terephthaloyl hydrazide by weight, and the other components are the same. The formula is shown in Table 1, and the performance test results are shown in Table 2.
[0053] Example 7
[0054] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material contains 1.0 part of terephthaloyl hydrazide by weight, and the other components are the same. The formula is shown in Table 1, and the performance test results are shown in Table 2.
[0055] Example 8
[0056] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material contains 0.5 parts of 3-methyl-6-(2-pyridyl)-1,2,4,5-tetrazine by weight, and the other components are the same. The formula is shown in Table 1, and the performance test results are shown in Table 2.
[0057] Example 9
[0058] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material contains 1.5 parts of 3-methyl-6-(2-pyridyl)-1,2,4,5-tetrazine by weight, and the other components are the same. The formula is shown in Table 1, and the test results are shown in Table 2.
[0059] Example 10
[0060] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, s-PB (JSR RB830, melting point 105° C.) 5 parts, the other components are the same, the formula is shown in Table 1, and the test results are shown in Table 2.
[0061] Embodiment 11
[0062] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, s-PB (JSR RB820, melting point 95° C.) 5 parts, the other components are the same, the formula is shown in Table 1, and the test results are shown in Table 2.
[0063] Example 12
[0064] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, contains 0.6 parts of sebacic acid dihydrazide and 1 part of 3,6-bis(4-hydroxyphenyl)-1,2,4,5-tetrazine, and the other components are the same. The formula is shown in Table 1, and the test results are shown in Table 2.
[0065] Comparative Example 1
[0066] A natural rubber compound material, the components of which are as follows, by weight: 100 parts of natural rubber, 55 parts of carbon black N220, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 0.5 parts of coupling agent si-69, 2.5 parts of sulfur, 1 part of accelerator CZ, the formula is shown in Table 1, and the performance test results are shown in Table 2.
[0067] Comparative Example 2
[0068] A natural rubber compound material, the components of which are as follows, by weight: 100 parts of natural rubber, 45 parts of carbon black N220, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 0.5 parts of coupling agent si-69, 2.5 parts of sulfur, 1 part of accelerator CZ, the formula is shown in Table 1, and the test results are shown in Table 2.
[0069] Comparative Example 3
[0070] A natural rubber compound material, the components of which are as follows, by weight: 100 parts of natural rubber, 35 parts of carbon black N220, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of antioxidant 4020, 0.5 parts of coupling agent si-69, 2.5 parts of sulfur, 1 part of accelerator CZ, the formula is shown in Table 1, and the test results are shown in Table 2.
[0071] Comparative Example 4
[0072] The difference from Example 1 is that the organic polymer reinforced natural rubber compound material does not contain 3-methyl-6-(2-pyridyl)-1,2,4,5-tetrazine, and the other components are the same. The formula is shown in Table 1, and the test results are shown in Table 2.
[0073] Comparative Example 5
[0074] The difference from Example 1 is that the organic polymer reinforced natural rubber compound material does not contain terephthaloyl hydrazide, and the other components are the same. The formula is shown in Table 1, and the test results are shown in Table 2.
[0075] Comparative Example 6
[0076] The difference from Example 1 is that the organic polymer reinforced natural rubber compound material does not contain terephthaloyl hydrazide and 3-methyl-6-(2-pyridyl)-1,2,4,5-tetrazine, and the other components are the same. The formula is shown in Table 1, and the test results are shown in Table 2.
[0077] Comparative Example 7
[0078] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, s-PB (JSR RB840, melting point 126°C) 10 parts, carbon black N220 55 parts, the other components are the same, the formula is shown in Table 1, and the test results are shown in Table 2.
[0079] Comparative Example 8
[0080] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, s-PB (JSR RB840, melting point 126°C) 5 parts, carbon black N220 40 parts, the other components are the same, the formula is shown in Table 1, and the test results are shown in Table 2.
[0081] Comparative Example 9
[0082] The difference from Example 1 is that an organic polymer reinforced natural rubber compound material, by weight, s-PB (JSR RB810, melting point 71° C.) 5 parts, the other components are the same, the formula is shown in Table 1, and the test results are shown in Table 2.
[0083] Table 1 Examples and Comparative Examples
[0084]
[0085]
[0086] Table 2 Performance comparison of examples and comparative examples
[0087]
[0088]
[0089] By comparing the performance of Examples 1, 2, and 3, it can be seen that the compression fatigue temperature rise of the material is consistent with the change trend of the number of reinforcing fillers. The more the number of reinforcing fillers, the higher the heat generation of the material. Although the heat generation of the material can be reduced by simply reducing the number of reinforcing fillers, it will also cause the performance of the material to deteriorate. Its tensile stress, hardness, high-temperature tensile strength and other properties will be significantly reduced, which cannot meet the actual use requirements.
[0090] It can be seen from the examples that the heat generation of the organic polymer reinforced natural rubber compound obtained by the scheme of the present invention is significantly reduced, and the compression fatigue heat generation is reduced to 15.9°C, and it can continue to maintain a high tensile stress, hardness, tensile strength, and elongation at break, and the high temperature performance is improved, and the high temperature tensile strength is increased to 13.9MPa; Combining Example 1 with Comparative Examples 4, 5, and 6, it can be seen that with the addition of natural rubber modifiers and organic polymer modifiers, the tensile stress and high temperature mechanical strength of the material are improved, and the heat generation is reduced, which is mainly due to the addition of modifiers Further improve the dispersion effect of carbon black reinforcing fillers; Combining Example 1 with Comparative Examples 7 and 8, it can be seen that when the organic polymer reinforced particles are mixed with carbon black reinforcing fillers, the organic polymer reinforced particles can be used to strengthen the carbon black reinforcing fillers. When the total amount of the reinforcing filler exceeds 60 parts by weight (65 parts in Comparative Example 7), the filler ratio is too large and cannot reduce the heat generation, and the actual heat generation increases slightly. When the total amount of the organic polymer reinforcing particles and the carbon black reinforcing filler is less than 50 parts by weight (45 parts in Comparative Example 8), the carbon black portion is reduced too much, causing the modulus of the material to drop to 2.3 MPa and the hardness to drop to 63, which cannot meet the use requirements of the material. Combining Example 1 with Comparative Example 9, it can be seen that when the melting point of the organic polymer reinforcing particles is lower than 90°C (the melting point of s-PB in Comparative Example 9 is 71°C), the reinforcing particles cannot maintain their crystalline structure at high temperatures, causing the high-temperature mechanical strength of the material to be significantly reduced to 11.2 MPa.
[0091] Based on the above performance, it can be seen that by adding organic polymer reinforcing particles to replace part of the reinforcing filler, and under the synergistic effect of the natural rubber modifier and the organic polymer modifier, the prepared organic polymer reinforced natural rubber compound material can continue to maintain high tensile stress, hardness, tensile strength, and elongation at break while significantly reducing heat generation, that is, this organic polymer reinforced natural rubber compound material can take into account the characteristics of high load-bearing and low heat generation. At the same time, due to the good compatibility of the organic polymer reinforcing particles with the natural rubber matrix and the unique reinforcement structure, the prepared organic polymer reinforced natural rubber compound material also has a significant improvement in high-temperature mechanical properties.
[0092] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to enumerate all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. An organic polymer reinforced natural rubber compound material, characterized in that: Its components are: The natural rubber is one of smoked sheet rubber and full latex standard rubber; the organic polymer reinforcing particles are syndiotactic 1,2-polybutadiene materials, and the melting point of syndiotactic 1,2-polybutadiene materials is 95-126°C; the natural rubber modifier is a dihydrazide compound; the organic polymer modifier is a tetrazine compound; the auxiliary agents are zinc oxide, stearic acid, antioxidant, coupling agent, sulfur and accelerator.
2. The organic polymer reinforced natural rubber compound material according to claim 1, characterized in that: The total amount of the organic polymer reinforcing particles and the carbon black reinforcing filler is 50 to 60 parts by weight.
3. The organic polymer reinforced natural rubber compound material according to claim 1 or 2, characterized in that: The natural rubber modifier is terephthaloyl hydrazide or sebacic acid dihydrazide.
4. The organic polymer reinforced natural rubber compound material according to claim 1 or 2, characterized in that: The organic polymer modifier is 3-methyl-6-(2-pyridyl)-1,2,4,5-tetrazine or 3,6-bis(4-hydroxyphenyl)-1,2,4,5-tetrazine.
5. The organic polymer reinforced natural rubber compound material according to claim 1, characterized in that: The auxiliary agent is 3-5 parts of zinc oxide, 2-3 parts of stearic acid, 1-3 parts of antioxidant, 0.5-2 parts of coupling agent, 1-4 parts of sulfur and 0.5-3 parts of accelerator.
6. The organic polymer reinforced natural rubber compound material according to claim 1 or 2, characterized in that: The carbon black reinforcing filler is one of carbon black N220, carbon black N330 and carbon black N550.
7. The organic polymer reinforced natural rubber compound material according to claim 1 or 5, characterized in that: The antioxidant is one of antioxidant 4010NA, antioxidant 4020, and antioxidant RD; the accelerator is one of accelerator NS, accelerator CZ, and accelerator DM; and the coupling agent is silane coupling agent Si-69.
8. A method for preparing the organic polymer reinforced natural rubber compound material according to claim 1, characterized in that: The specific steps are as follows: 1) One-stage mixing: natural rubber and dihydrazide compounds are put into an internal mixer and mixed at a speed of 30-45 rpm for 90-100 seconds, organic polymer modifiers and tetrazine modifiers are put into the internal mixer and mixed for 100-120 seconds, zinc oxide, stearic acid, antioxidant, coupling agent and carbon black reinforcing filler are added into the internal mixer, and the mass is lifted and pressed every 30-40 seconds. When the temperature of the rubber material reaches 125-130°C, the rubber material is continuously mixed for 80-95 seconds and then discharged; 2) Second stage mixing: the first stage mixed rubber of step 2) is put into an internal mixer together with sulfur and an accelerator, and mixed at a speed of 20-30 rpm. When the temperature of the rubber material reaches 100-115° C., the rubber material is discharged and placed to cool, thereby obtaining a natural rubber mixed rubber material.
Citation Information
Cited By
High-performance modified natural rubber material for sounding balloon and preparation method of high-performance modified natural rubber material
CN121136220A
High-performance modified natural rubber material for sounding balloon and preparation method thereof
CN121136220B