Epoxy molding compound capable of reducing hygroscopicity and preparation method thereof
The method of coating epoxy resin with carbon dot fluororesin solves the problem of high hygroscopicity of epoxy plastic sealing materials, reduces the risk of water molecules entering the chip, improves the mechanical properties and bonding capabilities of the materials, and reduces production costs. .
Patent Information
- Application Number
- CN202411385128.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
The high hygroscopicity of existing epoxy plastic sealing materials leads to peeling and corrosion of the chips inside the packaging products, and the treatment methods lead to a decrease in the flexibility of the material, increasing processing difficulty and increasing cost.
Chemically modified fluororesin is used to prepare carbon dot structures, and epoxy resin is coated with carbon dot fluororesin to reduce hygroscopy and maintain material flexibility. Epoxy plastic sealing materials are prepared using silicon micropowder, curing agent, coloring agent, etc.
Effectively reduces water molecules invading the chip, reduces the risk of corrosion, improves the mechanical properties and bonding capabilities of materials, reduces production costs, and is simple in process.
Smart Images

Figure CN119039738A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of epoxy resin chemical raw materials, and in particular to an epoxy molding compound used for packaging semiconductor devices such as transistors, power devices, integrated circuits, etc., and a preparation method thereof. Background Art
[0002] Epoxy molding compound, also known as epoxy molding compound (EMC), has excellent electrical properties, high heat resistance, good adhesion, strong corrosion resistance, high reliability and low cost. About 97% of semiconductor devices have been encapsulated with epoxy molding compound, including transistors, power devices, integrated circuits, etc.
[0003] Epoxy molding compound is mainly made of more than ten components such as epoxy resin, curing agent, inorganic filler, accelerator, etc. Since epoxy molding compound is a non-airtight packaging material with large molecular spacing, during the working process, water molecules can not only penetrate the packaging layer through the resin itself to reach the chip, but also penetrate through the interface between the resin and the lead frame to reach the chip, that is, epoxy molding compound has a high hygroscopicity.
[0004] The high hygroscopicity of epoxy molding compounds can cause internal peeling of packaged products or cracking of packaged parts. If the epoxy molding compound contains ionic impurities, the entry of water molecules can also cause electrochemical reactions and corrode the aluminum wiring on the chip.
[0005] In order to solve the problem of high hygroscopicity of epoxy molding compound, the art usually selects epoxy resin with low hygroscopicity as the base material, for example, epoxy resin with high cross-linking density, or adds hydrophobic filler to the base material. However, the above treatment will lead to decreased flexibility and increased brittleness of epoxy molding compound. The increased brittleness of the material may make it more prone to cracking or mechanical damage during use, and at the same time cause problems such as increased processing difficulty and increased cost.
[0006] Therefore, how to overcome the defects of existing epoxy molding compounds such as high hygroscopicity is a technical problem to be solved urgently in this field. Summary of the invention
[0007] The present invention solves the technical problem of high hygroscopicity of existing epoxy molding compounds, and provides an epoxy molding compound capable of reducing hygroscopicity and a preparation method thereof. The prepared epoxy molding compound can reduce the intrusion of water molecules and cause chip corrosion, while maintaining good material flexibility, and is easy to process and has low production cost.
[0008] The present invention provides an epoxy molding compound, which is prepared by mixing the following raw materials in percentage by mass:
[0009] Silica powder 87-90%, epoxy resin 3-4%, fluororesin 3-4%, curing agent 3-4%, colorant 0-1%, release agent 0-1%, accelerator 0-1%, other additives 0-1%.
[0010] Preferably, the epoxy resin is a crystalline bisphenol A epoxy resin or a biphenyl epoxy resin.
[0011] Preferably, the fluororesin is PVDF or FEVE fluororesin.
[0012] Preferably, the curing agent is a dicyclopentadiene phenolic resin or a phenol-phenyl alkyl phenolic resin.
[0013] Preferably, the colorant is carbon black.
[0014] Preferably, the release agent is natural wax or synthetic wax.
[0015] Preferably, the accelerator is triphenylphosphine.
[0016] Preferably, the other auxiliary agent is amino silicone oil or siloxane.
[0017] The preparation method of the epoxy molding compound provided by the present invention comprises the following steps:
[0018] Weigh the amount of silicon powder, epoxy resin, fluororesin, curing agent, colorant, release agent, accelerator and other additives according to the ratio of the epoxy molding compound;
[0019] The epoxy resin and the fluororesin are mixed and reacted to prepare the carbon dot fluororesin coated epoxy resin;
[0020] The epoxy resin coated with carbon dot fluorine resin is fully mixed with the curing agent, silicon powder, colorant, release agent, accelerator and other additives to obtain a mixture;
[0021] The mixture is placed on a double-roll mill at 125° C. to 45° C. for 30 minutes, and then cooled and crushed to obtain a powdered epoxy molding compound;
[0022] The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
[0023] Preferably, the preparation method of the carbon dot fluororesin coated epoxy resin comprises the following steps:
[0024] The fluororesin is placed in a polytetrafluoroethylene reactor, and heated and pressurized to form a fluororesin carbon dot solution;
[0025] Dissolving the epoxy resin in ethyl acetate solution and placing it in a constant flow pump;
[0026] The fluororesin carbon dot solution was added dropwise to the mixed solution of the epoxy resin solution and the ethyl acetate solution at a rate of 60 mL / h to react, and after the reaction was completed, suction filtration was performed to obtain a reactant;
[0027] The reactants were washed with deionized water to remove byproducts and unreacted products in the reaction, and then dried at 70° C. to obtain the carbon-dot fluorine resin-coated epoxy resin.
[0028] Preferably, the particle size of the fluororesin on the surface of the epoxy resin coated with the carbon dot fluororesin is less than 10 nm.
[0029] Preferably, the fluororesin is placed in a polytetrafluoroethylene reactor, heated to 170° C. to 190° C., maintained at a constant temperature for 5 to 7 hours, and then naturally cooled at room temperature to obtain the fluororesin carbon dot solution.
[0030] Since epoxy molding compound is a non-airtight packaging material with large molecular spacing, during operation, water molecules can not only penetrate through the resin itself to reach the chip, but also penetrate through the interface between the resin and the lead frame to reach the chip. If the epoxy molding compound also contains ionic impurities, the entry of water molecules will cause electrochemical reactions and corrode the aluminum wiring on the chip. Therefore, it is very important to improve the moisture resistance of epoxy molding compound.
[0031] In order to solve the above problem, the present invention firstly adopts a chemical method to modify the fluororesin, that is, to prepare a fluororesin with a carbon dot structure, and then introduces the fluororesin with the carbon dot structure to coat the epoxy resin. Since there are a large number of hydrophobic fluorine groups on the fluororesin molecular chain, the epoxy resin is coated with the fluororesin to isolate the hydrophilic groups and polar groups on the epoxy resin from contact with water molecules, which greatly reduces the contact between the epoxy molding compound and water molecules. That is, the epoxy molding compound prepared by the epoxy resin coated with the carbon dot fluororesin can not only reduce its own hygroscopicity and moisture permeability, but also reduce the phenomenon of internal chip corrosion caused by water molecules. It is also easy to disperse, so that the product surface has a good dispersion effect and is easy to bond; it also has low toxicity, simple process and low production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a schematic diagram of the process flow of the method for preparing the epoxy molding compound. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the following specific embodiments are only used to explain the present invention and do not constitute a limitation to the present invention.
[0034] The epoxy molding compound provided by the present invention is prepared by mixing the following raw materials by weight percentage:
[0035] Silica powder 87-90%, epoxy resin 3-4%, fluororesin 3-4%, curing agent 3-4%, colorant 0-1%, release agent 0-1%, accelerator 0-1%, other additives 0-1%.
[0036] Among them, the epoxy resin is preferably a crystalline bisphenol A epoxy resin or a biphenyl epoxy resin. The fluororesin is preferably PVDF or FEVE fluororesin. The curing agent is preferably a dicyclopentadiene phenolic resin or a phenol-phenyl alkyl phenolic resin. The colorant is preferably carbon black. The release agent is preferably a natural wax or a synthetic wax. The accelerator is preferably triphenylphosphine. Other auxiliary agents can be coupling agents, preferably amino silicone oil or siloxane.
[0037] The preparation method of the epoxy molding compound provided by the present invention comprises the following steps:
[0038] Weigh the amount of silicon powder, epoxy resin, fluororesin, curing agent, colorant, release agent, accelerator and other additives according to the ratio of the epoxy molding compound;
[0039] The epoxy resin and the fluororesin are mixed and reacted to prepare the carbon dot fluororesin coated epoxy resin;
[0040] The epoxy resin coated with carbon dot fluororesin is fully mixed with the curing agent, silicon powder, colorant, release agent, accelerator and other additives to obtain a mixture;
[0041] The mixture is placed on a double-roll mill at 125° C. to 45° C. for 30 minutes, and then cooled and crushed to obtain a powdered epoxy molding compound;
[0042] The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
[0043] The preparation method of the carbon dot fluorine resin coated epoxy resin comprises the following steps:
[0044] placing the fluororesin in a polytetrafluoroethylene reactor, heating and pressurizing to form a fluororesin carbon dot solution;
[0045] Dissolving the epoxy resin in ethyl acetate solution and placing it in a constant flow pump;
[0046] The fluororesin carbon dot solution was added dropwise to the mixed solution of the epoxy resin and the ethyl acetate solution at a rate of 60 mL / h to react, and after the reaction was completed, suction filtration was performed to obtain a reactant;
[0047] The reactants were washed with deionized water to remove byproducts and unreacted products in the reaction, and dried at 70° C. to obtain epoxy resin coated with carbon dot fluororesin. The particle size of fluororesin on the surface of the epoxy resin coated with carbon dot fluororesin was less than 10 nm.
[0048] The fluororesin is placed in a polytetrafluoroethylene reactor, heated to 170° C. to 190° C., kept at a constant temperature for 5 to 7 hours, and then naturally cooled at room temperature to obtain the fluororesin carbon dot solution.
[0049] The present invention is further described below by way of examples. According to the raw material ratio of the epoxy molding compound of the present invention, the raw material ratios (mass percentage) of the following five embodiments of the present invention and two comparative examples of the prior art are given, as shown in Table 1:
[0050] Table 1
[0051]
[0052] The raw material dosages of the two comparative examples in Table 1 are similar to those of the epoxy molding compound provided by the present invention, except that the raw material fluororesin is missing.
[0053] The samples of the examples were prepared according to the preparation method of the epoxy molding compound proposed in the present invention. Figure 1 The raw material ratios of the embodiments and comparative examples are shown in Table 1.
[0054] Example 1
[0055] According to the ratio of epoxy molding compound, weigh 87 grams of silicon powder, 4 grams of crystalline bisphenol A epoxy resin, 3.5 grams of PVDF fluororesin, 4 grams of dicyclopentadiene phenolic resin, 1 gram of carbon black and 0.5 grams of natural wax.
[0056] The epoxy resin and the fluororesin are mixed and reacted to prepare the carbon point fluororesin coated epoxy resin, and the preparation method comprises the following steps:
[0057] 3.5 grams of PVDF fluororesin was placed in a stainless steel autoclave lined with polytetrafluoroethylene, the autoclave was tightened and placed in an oven, heated to 180°C, and kept at a constant temperature for 6 hours, then the autoclave was taken out and placed at room temperature to cool naturally, and the solution was taken out after cooling to obtain a fluororesin carbon dot solution.
[0058] Dissolve 4 grams of crystalline bisphenol A epoxy resin in ethyl acetate solution and place it in a constant flow pump.
[0059] The fluororesin carbon dot solution was added dropwise to the mixed solution of the epoxy resin and the ethyl acetate solution at a rate of 60 mL / h for reaction. At this time, the solubility of the fluororesin was reduced, so that the fluororesin was precipitated and coated on the surface of the epoxy resin. After the reaction was completed, suction filtration was performed to obtain a reactant.
[0060] The reactants were washed with deionized water to remove byproducts and unreacted products in the reaction, and dried at 70° C. to obtain epoxy resin coated with carbon dot fluororesin. The particle size of fluororesin on the surface of the epoxy resin coated with carbon dot fluororesin was less than 10 nm.
[0061] The prepared carbon-dot fluorine resin-coated epoxy resin was fully mixed with 87 grams of silicon micropowder, 4 grams of dicyclopentadiene phenolic resin, 1 gram of carbon black, and 0.5 grams of a release agent to obtain a mixture.
[0062] The mixture is placed on a double-roll open mill at 125° C. to 45° C. for 30 minutes of mixing, and then cooled and crushed to obtain a powdered epoxy molding compound.
[0063] The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
[0064] Example 2
[0065] According to the ratio of epoxy molding compound, weigh 88.5 grams of silicon micropowder, 3.5 grams of biphenyl epoxy resin, 4 grams of FEVE fluororesin, 3 grams of phenol-phenyl alkyl phenolic resin and 1 gram of synthetic wax.
[0066] The epoxy resin and the fluororesin are mixed and reacted to prepare the carbon point fluororesin coated epoxy resin, and the preparation method comprises the following steps:
[0067] Place 4 grams of FEVE fluororesin in a stainless steel autoclave lined with polytetrafluoroethylene, tighten the autoclave and place it in an oven, heat it to 190°C, keep the temperature constant for 5 hours, take out the autoclave, and place it at room temperature to cool naturally. After cooling, take out the solution to obtain a fluororesin carbon dot solution.
[0068] Dissolve 3.5 g of biphenyl epoxy resin in ethyl acetate solution and place it in a constant flow pump.
[0069] The fluororesin carbon dot solution was added dropwise to the mixed solution of the epoxy resin and the ethyl acetate solution at a rate of 60 mL / h for reaction. At this time, the solubility of the fluororesin was reduced, so that the fluororesin was precipitated and coated on the surface of the epoxy resin. After the reaction was completed, suction filtration was performed to obtain a reactant.
[0070] The reactants were washed with deionized water to remove byproducts and unreacted products in the reaction, and dried at 70° C. to obtain epoxy resin coated with carbon dot fluororesin. The particle size of fluororesin on the surface of the epoxy resin coated with carbon dot fluororesin was less than 10 nm.
[0071] The prepared carbon-dot fluorine resin-coated epoxy resin was fully mixed with 88.5 g of silica powder, 3 g of phenol-phenyl alkyl phenolic resin, and 1 g of synthetic wax to obtain a mixture.
[0072] The mixture is placed on a double-roll open mill at 125° C. to 45° C. for 30 minutes of mixing, and then cooled and crushed to obtain a powdered epoxy molding compound.
[0073] The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
[0074] Example 3
[0075] According to the ratio of epoxy molding compound, weigh 90 grams of silicon powder, 3 grams of crystalline bisphenol A epoxy resin, 3 grams of FEVE fluororesin, 3.5 grams of phenol-phenyl alkyl phenolic resin, and 0.5 grams of carbon black.
[0076] The epoxy resin and the fluororesin are mixed and reacted to prepare the carbon point fluororesin coated epoxy resin, and the preparation method comprises the following steps:
[0077] Place 3 grams of FEVE fluororesin in a stainless steel autoclave lined with polytetrafluoroethylene, tighten the autoclave and place it in an oven, heat it to 170°C, keep the temperature constant for 7 hours, take out the autoclave, and place it at room temperature to cool naturally. After cooling, take out the solution to obtain a fluororesin carbon dot solution.
[0078] Dissolve 3 grams of crystalline bisphenol A epoxy resin in ethyl acetate solution and place it in a constant flow pump.
[0079] The fluororesin carbon dot solution was added dropwise to the mixed solution of the epoxy resin and the ethyl acetate solution at a rate of 60 mL / h for reaction. At this time, the solubility of the fluororesin was reduced, so that the fluororesin was precipitated and coated on the surface of the epoxy resin. After the reaction was completed, suction filtration was performed to obtain a reactant.
[0080] The reactants were washed with deionized water to remove byproducts and unreacted products in the reaction, and dried at 70° C. to obtain epoxy resin coated with carbon dot fluororesin. The particle size of fluororesin on the surface of the epoxy resin coated with carbon dot fluororesin was less than 10 nm.
[0081] The prepared carbon-dot fluorine resin-coated epoxy resin was fully mixed with 90 g of silica powder, 3.5 g of phenol-phenyl alkyl phenolic resin, and 0.5 g of carbon black to obtain a mixture.
[0082] The mixture is placed on a double-roll open mill at 125° C. to 45° C. for 30 minutes of mixing, and then cooled and crushed to obtain a powdered epoxy molding compound.
[0083] The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
[0084] Example 4
[0085] According to the ratio of epoxy molding compound, weigh 89 grams of silicon micropowder, 3 grams of biphenyl epoxy resin, 3 grams of PVDF fluororesin, 3 grams of dicyclopentadiene phenolic resin, 0.5 grams of natural wax, 0.5 grams of triphenylphosphine, and 1 gram of amino silicone oil.
[0086] The epoxy resin and the fluororesin are mixed and reacted to prepare the carbon point fluororesin coated epoxy resin, and the preparation method comprises the following steps:
[0087] The PVDF fluororesin 3 was placed in a stainless steel autoclave lined with polytetrafluoroethylene, the autoclave was tightened and placed in an oven, heated to 180°C, and kept at a constant temperature for 6 hours, then the autoclave was taken out and placed at room temperature to cool naturally, and the solution was taken out after cooling to obtain a fluororesin carbon dot solution.
[0088] Dissolve 3 grams of biphenyl epoxy resin in ethyl acetate solution and place it in a constant flow pump.
[0089] The fluororesin carbon dot solution was added dropwise to the mixed solution of the epoxy resin and the ethyl acetate solution at a rate of 60 mL / h for reaction. At this time, the solubility of the fluororesin was reduced, so that the fluororesin was precipitated and coated on the surface of the epoxy resin. After the reaction was completed, suction filtration was performed to obtain a reactant.
[0090] The reactants were washed with deionized water to remove byproducts and unreacted products in the reaction, and dried at 70° C. to obtain epoxy resin coated with carbon dot fluororesin. The particle size of fluororesin on the surface of the epoxy resin coated with carbon dot fluororesin was less than 10 nm.
[0091] The prepared carbon-dot fluorine resin-coated epoxy resin was fully mixed with 89 grams of silicon micropowder, 3 grams of dicyclopentadiene phenolic resin, 0.5 grams of natural wax, 0.5 grams of triphenylphosphine, and 1 gram of amino silicone oil to obtain a mixture.
[0092] The mixture is placed on a double-roll open mill at 125° C. to 45° C. for 30 minutes of mixing, and then cooled and crushed to obtain a powdered epoxy molding compound.
[0093] The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
[0094] Example 5
[0095] According to the ratio of epoxy molding compound, weigh 87 grams of silicon powder, 3 grams of biphenyl epoxy resin, 4 grams of PVDF fluororesin, 3 grams of dicyclopentadiene phenolic resin, 1 gram of carbon black, 0.5 grams of natural wax, 1 gram of triphenylphosphine, and 0.5 grams of siloxane.
[0096] The epoxy resin and the fluororesin are mixed and reacted to prepare the carbon point fluororesin coated epoxy resin, and the preparation method comprises the following steps:
[0097] Place 4 grams of PVDF fluororesin in a stainless steel autoclave lined with polytetrafluoroethylene, tighten the autoclave and place it in an oven, heat it to 180°C, keep the temperature constant for 6 hours, take out the autoclave, and place it at room temperature to cool naturally. After cooling, take out the solution to obtain a fluororesin carbon dot solution.
[0098] Dissolve 3 grams of biphenyl epoxy resin in ethyl acetate solution and place it in a constant flow pump.
[0099] The fluororesin carbon dot solution was added dropwise to the mixed solution of the epoxy resin and the ethyl acetate solution at a rate of 60 mL / h for reaction. At this time, the solubility of the fluororesin was reduced, so that the fluororesin was precipitated and coated on the surface of the epoxy resin. After the reaction was completed, suction filtration was performed to obtain a reactant.
[0100] The reactants were washed with deionized water to remove byproducts and unreacted products in the reaction, and dried at 70° C. to obtain epoxy resin coated with carbon dot fluororesin. The particle size of fluororesin on the surface of the epoxy resin coated with carbon dot fluororesin was less than 10 nm.
[0101] The prepared carbon-dot fluorine resin-coated epoxy resin was fully mixed with 87 grams of silica powder, 3 grams of dicyclopentadiene phenolic resin, 1 gram of carbon black, 0.5 grams of natural wax, 1 gram of triphenylphosphine, and 0.5 grams of siloxane to obtain a mixture.
[0102] The mixture is placed on a double-roll open mill at 125° C. to 45° C. for 30 minutes of mixing, and then cooled and crushed to obtain a powdered epoxy molding compound.
[0103] The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
[0104] The present invention uses epoxy resin coated with carbon dot fluororesin and curing agent as a matrix, silicon powder as a filler, and adds colorant, release agent, accelerator and other auxiliary agents, and fully mixes with a high-speed stirrer to obtain a mixture. Since the particle size of the carbon dot fluororesin coated on the surface of the epoxy resin prepared by the present invention is controlled to be less than 10nm, it not only has the hydrophobic property of fluororesin, plays a role in reducing the water absorption of the plastic packaging material, but also is easy to adhere to the surface of the electronic device and is not easy to peel off.
[0105] The samples of the comparative examples are prepared according to the raw material dosage ratios of the two comparative examples in Table 1:
[0106] Comparative Example 1
[0107] According to the ratio of the existing epoxy molding compound, 87 grams of silicon powder, 5 grams of crystalline bisphenol A epoxy resin, 4 grams of dicyclopentadiene phenolic resin, 1 gram of carbon black, 1 gram of natural wax, 1 gram of triphenylphosphine and 1 gram of siloxane were weighed.
[0108] The above epoxy resin and dicyclopentadiene phenolic resin matrix are used, the above silicon powder is used as filler, a colorant, a release agent, a promoter and other auxiliary agents are added, and they are fully mixed by a high-speed stirrer to obtain a mixture.
[0109] The mixture is placed on a double-roll open mill at 125°C to 45°C for 30 minutes of mixing, and then cooled and crushed to obtain a powdered epoxy molding compound. The obtained powder is made into a cake-shaped epoxy molding compound of a certain specification using a cake-making machine.
[0110] Comparative Example 2
[0111] According to the ratio of the existing epoxy molding compound, 90 grams of silicon powder, 4 grams of biphenyl epoxy resin, 3.5 grams of phenol-phenyl alkyl phenolic resin, 0.5 grams of carbon black, 1 gram of synthetic wax and 1 gram of triphenylphosphine were weighed.
[0112] The above-mentioned biphenyl epoxy resin and phenol-phenyl alkyl phenolic resin matrix are used as the above-mentioned silicon powder as filler, and colorant, release agent, accelerator and other auxiliary agents are added, and they are fully mixed by a high-speed stirrer to obtain a mixture.
[0113] The mixture is placed on a double-roll open mill at 125° C. to 45° C. for 30 minutes of mixing, and then cooled and crushed to obtain a powdered epoxy molding compound.
[0114] The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
[0115] The performance of samples of five embodiments of the present invention and two comparative examples are tested below.
[0116] According to the test method standard for epoxy molding compounds for electronic packaging (GB / T 40564-2021), the following performance parameters of epoxy molding compounds are tested:
[0117] 1) Water absorption rate;
[0118] 2) Bending strength test: Epoxy plastic encapsulation material shall be tested according to the test method standard for thermal conductivity of fiber reinforced plastics (GB / T3139-2005);
[0119] 3) Thermal conductivity.
[0120] The testing equipment and procedures are as specified in GB / T 40564-2021.
[0121] The test results of the embodiments of the present invention and the comparative examples are shown in Table 2:
[0122] Table 2
[0123]
[0124] Since there are a large number of hydrophobic fluorine groups on the fluororesin molecular chain, the structure prevents the hydrophilic groups and polar groups on the epoxy resin from contacting with water molecules in large quantities. A layer of carbon dot fluororesin is constructed, which can not only greatly reduce the contact between the product and water molecules, but also because the carbon dots are extremely small in size, their special structure can improve the mechanical properties and bonding ability of the product to a certain extent.
[0125] As shown in Table 2, without affecting the bending strength and thermal conductivity of the epoxy molding compound, the water absorption rate of the example sample is significantly lower than that of the comparative example sample, and the mechanical properties of the example are also significantly improved. By coating the carbon point fluororesin, the water absorption rate of the epoxy molding compound can be reduced.
[0126] The present invention adopts a chemical method to modify the fluororesin, that is, to prepare a fluororesin with a carbon dot structure, and then the fluororesin with the carbon dot structure is coated with an epoxy resin. This can not only reduce the hygroscopicity and moisture permeability of the epoxy molding compound itself, but also reduce the phenomenon of internal chip corrosion caused by water molecules. It is also easy to disperse, so that the product surface has a good dispersion effect and is easy to bond. It also has low toxicity, simple process and low production cost.
[0127] It should be noted that the terms used in this specification are only for describing specific embodiments and are not intended to limit the present invention. Unless otherwise specifically stated, the relative arrangement of the technical features and steps, numerical expressions and numerical values described in these embodiments do not limit the scope of protection of the present invention.
[0128] The techniques, methods and devices known to those skilled in the art are not discussed in detail in this specification, but where appropriate, the techniques, methods and devices should be considered as part of this specification. Any specific values in this specification should be interpreted as being merely exemplary and not limiting the present invention.
[0129] The above description is only a specific implementation of the present invention. It should be pointed out that any modification, equivalent substitution and change made within the spirit and framework of the present invention should be included in the protection scope of the present invention.
Claims
1. An epoxy molding compound, prepared by the following raw materials in percentage by mass: Silica powder 87-90%, epoxy resin 3-4%, fluororesin 3-4%, curing agent 3-4%, colorant 0-1%, release agent 0-1%, accelerator 0-1%, other additives 0-1%.
2. The epoxy molding compound according to claim 1, It is characterized in that The epoxy resin is a crystalline bisphenol A epoxy resin or a biphenyl epoxy resin.
3. The epoxy molding compound as claimed in claim 1, It is characterized in that The fluororesin is PVDF or FEVE fluororesin.
4. The epoxy molding compound as claimed in claim 1, It is characterized in that The curing agent is dicyclopentadiene type phenolic resin or phenol-phenyl alkyl type phenolic resin.
5. The epoxy molding compound as claimed in claim 1, It is characterized in that The colorant is carbon black.
6. The epoxy molding compound according to claim 1, It is characterized in that The release agent is natural wax or synthetic wax.
7. The epoxy molding compound according to claim 1, It is characterized in that The accelerator is triphenylphosphine.
8. The epoxy molding compound as claimed in claim 1, It is characterized in that The coupling agent is amino silicone oil or siloxane.
9. The method for preparing the epoxy molding compound according to any one of claims 1 to 8, comprising the following steps: Weigh the amount of silicon powder, epoxy resin, fluororesin, curing agent, colorant, release agent, accelerator and other additives according to the ratio of the epoxy molding compound; The epoxy resin and the fluororesin are mixed and reacted to prepare the carbon dot fluororesin coated epoxy resin; The epoxy resin coated with carbon dot fluorine resin is fully mixed with the curing agent, silicon powder, colorant, release agent, accelerator and other additives to obtain a mixture; The mixture is placed on a double-roll mill at 125° C. to 45° C. for 30 minutes, and then cooled and crushed to obtain a powdered epoxy molding compound; The powdered epoxy molding compound is made into a cake-shaped epoxy molding compound of a certain specification.
10. The method for preparing the epoxy molding compound according to claim 9, It is characterized in that The preparation method of the carbon point fluorine resin coated epoxy resin comprises the following steps: The fluororesin is placed in a polytetrafluoroethylene reactor, and heated and pressurized to form a fluororesin carbon dot solution; Dissolving the epoxy resin in ethyl acetate solution and placing it in a constant flow pump; The fluororesin carbon dot solution was added dropwise to the mixed solution of the epoxy resin solution and the ethyl acetate solution at a rate of 60 mL / h to react, and after the reaction was completed, suction filtration was performed to obtain a reactant; The reactants were washed with deionized water to remove byproducts and unreacted products in the reaction, and then dried at 70° C. to obtain the carbon-dot fluorine resin-coated epoxy resin.
11. The method for preparing the epoxy molding compound according to claim 10, It is characterized in that The particle size of the fluororesin on the surface of the epoxy resin coated with the carbon point fluororesin is less than 10 nm.
12. The method for preparing the epoxy molding compound according to claim 10, It is characterized in that The fluororesin is placed in a polytetrafluoroethylene reaction kettle, heated to 170° C. to 190° C., maintained at a constant temperature for 5 to 7 hours, and then naturally cooled at room temperature to obtain the fluororesin carbon dot solution.