Engineering plastic for communication optical cable and preparation method thereof

By blending modified nylon 6 and polymethyl methacrylate and modifying the surface of raptosite, an engineering plastic for communication optical cables with excellent wear resistance and tensile properties was prepared. This solved the problem of insufficient wear resistance and tensile properties of plastic materials in the existing technology, and enabled stable transmission of optical cables in complex environments.

CN119039778AInactive Publication Date: 2024-11-29HEBEI SHANGHUA NEW MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411533719.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The plastic materials used in existing communication optical cables do not perform well in terms of abrasion resistance and tensile properties, and cannot meet the requirements for stable operation and high-performance transmission in complex environments.

Method used

Engineering plastics with excellent wear resistance and tensile properties are prepared by using modified nylon 6, polymethyl methacrylate and polyurethane elastomer as components, through blending and surface modification treatment. Specifically, the preparation method of modified nylon 6 and surface modification treatment of attapulgite are included.

Benefits of technology

It significantly improves the wear resistance and tensile properties of engineering plastics for communication optical cables, meeting the requirements for stable operation in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of optical cable materials, and provides engineering plastic for communication optical cables and a preparation method thereof.The engineering plastic for the communication optical cables is prepared from, by weight, 50-70 parts of modified nylon 6, 10-15 parts of polyethylene glycol terephthalate, 15-25 parts of rectorite, 1-5 parts of compatilizer, 1-3 parts of antioxidant and 0.5-1.5 parts of lubricant; the raw materials of the modified nylon 6 comprise polymethyl methacrylate and nylon 6. According to the technical scheme, the problems of poor wear resistance and poor tensile property of the engineering plastic for the communication optical cable in related technologies are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical cable materials, and in particular to an engineering plastic for communication optical cables and a preparation method thereof. Background Art

[0002] Communication optical cable is a communication line composed of several optical fibers in a certain way to realize the transmission of optical signals. Communication optical cable has the remarkable characteristics of large transmission capacity, long transmission distance and low signal attenuation. It can stably transmit a large amount of information, including voice, data, images and videos, over long distances and at high rates. In communication optical cables, plastics are often used as sheath materials, which directly affect the performance, reliability and service life of communication optical cables. The plastic materials currently used for communication optical cables perform poorly in terms of wear resistance and mechanical properties, and cannot meet the stable operation and high-performance transmission requirements of communication optical cables in complex environments. Therefore, it is of great practical significance to develop an engineering plastic with good wear resistance and excellent tensile properties as the sheath material of communication optical cables. Summary of the invention

[0003] The present invention provides an engineering plastic for communication optical cables and a preparation method thereof, which solves the problems of poor wear resistance and poor tensile properties of the engineering plastic for communication optical cables in the related art.

[0004] The technical solution of the present invention is as follows: The present invention provides an engineering plastic for communication optical cable, comprising the following components in parts by weight: 50-70 parts of modified nylon 6, 10-15 parts of polyethylene terephthalate, 15-25 parts of rectorite, 1-5 parts of compatibilizer, 1-3 parts of antioxidant, 0.5-1.5 parts of lubricant; The raw materials of the modified nylon 6 include polymethyl methacrylate and nylon 6.

[0005] As a further technical solution, the weight ratio of the nylon 6 to the polymethyl methacrylate is 5-9:1.

[0006] When the weight ratio of nylon 6 and polymethyl methacrylate is 5~9:1, the wear resistance and tensile properties of engineering plastics used for communication optical cables can be further improved.

[0007] As a further technical solution, the preparation method of the modified nylon 6 comprises the following steps: melting the polymethyl methacrylate, adding nylon 6, blending, cooling, and granulating to obtain modified nylon 6.

[0008] As a further technical solution, during the melting, the temperature is 150-170° C. and the time is 1-2 hours.

[0009] As a further technical solution, the raw material of the modified nylon 6 also includes polyurethane elastomer.

[0010] Nylon 6 is modified by using polymethyl methacrylate and polyurethane elastomer. By using the three together, the tensile properties can be ensured while further improving the wear resistance of engineering plastics used in communication optical cables.

[0011] As a further technical solution, the weight ratio of nylon 6, polymethyl methacrylate and polyurethane elastomer is 50:5~8:2~5.

[0012] When the weight ratio of nylon 6, polymethyl methacrylate and polyurethane elastomer is 50:5~8:2~5, the wear resistance of engineering plastics used for communication optical cables can be further improved.

[0013] As a further technical solution, the preparation method of the modified nylon 6 comprises the following steps: after the polymethyl methacrylate and the polyurethane elastomer are blended and melted, nylon 6 is added, dispersed evenly, cooled, and granulated to obtain modified nylon 6.

[0014] As a further technical solution, during the blending and melting, the temperature is 170-180° C. and the time is 1-2 hours.

[0015] As a further technical solution, the rectorite is modified rectorite, and the raw materials of the modified rectorite include rectorite, potassium oleate and dioctadecyl dimethyl ammonium chloride.

[0016] Surface modification of rectorite using potassium oleate and dioctadecyl dimethyl ammonium chloride can reduce the agglomeration of rectorite, thereby improving the effective combination of rectorite with other components and enhancing the overall structural stability of engineering plastics, thereby further improving the wear resistance of engineering plastics used for communication optical cables.

[0017] As a further technical solution, the preparation method of the modified rectorite includes the following steps: dissolving the potassium oleate and the dioctadecyl dimethyl ammonium chloride in ethanol to obtain a mixed solution, adding the rectorite to the mixed solution, dispersing evenly, concentrating, and drying to obtain the modified rectorite.

[0018] As a further technical solution, the weight ratio of the rectorite, potassium oleate and dioctadecyl dimethyl ammonium chloride is 8-18:1:1.

[0019] When the weight ratio of rectorite, potassium oleate and dioctadecyl dimethyl ammonium chloride is 8-18:1:1, the wear resistance of engineering plastics used for communication optical cables can be further improved.

[0020] As a further technical solution, the mass fraction of the mixed solution is 15%~20%.

[0021] As a further technical solution, the compatibilizer is one or more of maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, and maleic anhydride grafted ethylene-vinyl acetate copolymer; the antioxidant is one or more of antioxidant 1010, antioxidant 168, and antioxidant 1076; and the lubricant is one or both of polyethylene wax and calcium stearate.

[0022] The present invention also provides a method for preparing engineering plastics for communication optical cables, comprising the following steps: blending the components in parts by weight, extruding and granulating, and obtaining the engineering plastics for communication optical cables.

[0023] As a further technical solution, during the extrusion, the temperature is 190-210°C.

[0024] The working principle and beneficial effects of the present invention are: In the present invention, the engineering plastics used for communication optical cables include modified nylon 6. By using polymethyl methacrylate to mix and modify nylon 6, the compatibility of nylon 6 with other components is improved, and the internal stability of the engineering plastics can be enhanced, thereby improving the wear resistance and tensile properties of the engineering plastics used for communication optical cables. In addition, the addition of rectorite can also improve the wear resistance and tensile properties of the engineering plastics used for communication optical cables. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the following embodiments and comparative examples, the model of nylon 6 is BFG10; the model of polyethylene terephthalate is 702MS; the particle size of rectorite is 400 mesh; the model of maleic anhydride grafted polyethylene is ZJ-800E; the model of polyethylene wax is LA-B10; the model of polymethyl methacrylate is SG-7; and the model of polyurethane elastomer is LP9062.

[0027] Example 1 An engineering plastic for communication optical cable, comprising the following components in parts by weight: 50 parts of modified nylon 6, 10 parts of polyethylene terephthalate, 15 parts of rectorite, 1 part of maleic anhydride grafted polyethylene, 1 part of antioxidant 1076, 0.5 parts of polyethylene wax; The raw materials of modified nylon 6 include 10 parts of polymethyl methacrylate and 40 parts of nylon 6; The preparation method of modified nylon 6 comprises the following steps: melting 10 parts of polymethyl methacrylate at 150° C. for 2 hours, adding 40 parts of nylon 6, blending, cooling, and granulating to obtain modified nylon 6; The method for preparing engineering plastics for communication optical cables comprises the following steps: blending the above components in parts by weight, extruding and granulating to obtain engineering plastics for communication optical cables; Among them, the extrusion temperature of zone one is 190°C, the extrusion temperature of zone two is 210°C, and the extrusion temperature of zone three is 200°C.

[0028] Example 2 An engineering plastic for communication optical cable, comprising the following components in parts by weight: 60 parts of modified nylon 6, 13 parts of polyethylene terephthalate, 20 parts of rectorite, 3 parts of maleic anhydride grafted polyethylene, 2 parts of antioxidant 1076, 1 part of polyethylene wax; The raw materials of modified nylon 6 include 12 parts of polymethyl methacrylate and 48 parts of nylon 6; The preparation method of modified nylon 6 comprises the following steps: melting 12 parts of polymethyl methacrylate at 160° C. for 1.5 hours, adding 48 parts of nylon 6, blending, cooling, and granulating to obtain modified nylon 6; The method for preparing engineering plastics for communication optical cables comprises the following steps: blending the above components in parts by weight, extruding and granulating to obtain engineering plastics for communication optical cables; Among them, the extrusion temperature of zone one is 190°C, the extrusion temperature of zone two is 210°C, and the extrusion temperature of zone three is 200°C.

[0029] Example 3 An engineering plastic for communication optical cable, comprising the following components in parts by weight: 70 parts of modified nylon 6, 15 parts of polyethylene terephthalate, 25 parts of rectorite, 5 parts of maleic anhydride grafted polyethylene, 3 parts of antioxidant 1076, 1.5 parts of polyethylene wax; The raw materials of modified nylon 6 include 14 parts of polymethyl methacrylate and 56 parts of nylon 6; The preparation method of modified nylon 6 comprises the following steps: melting 14 parts of polymethyl methacrylate at 170° C. for 1 hour, adding 56 parts of nylon 6, blending, cooling, and granulating to obtain modified nylon 6; The method for preparing engineering plastics for communication optical cables comprises the following steps: blending the above components in parts by weight, extruding and granulating to obtain engineering plastics for communication optical cables; Among them, the extrusion temperature of zone one is 190°C, the extrusion temperature of zone two is 210°C, and the extrusion temperature of zone three is 200°C.

[0030] Example 4 The only difference between this embodiment and embodiment 2 is that in this embodiment, the raw materials of modified nylon 6 include 5 parts of polymethyl methacrylate and 55 parts of nylon 6.

[0031] Example 5 The only difference between this embodiment and embodiment 2 is that in this embodiment, the raw materials of modified nylon 6 include 6 parts of polymethyl methacrylate and 54 parts of nylon 6.

[0032] Example 6 The only difference between this embodiment and embodiment 2 is that, in this embodiment, the raw materials of modified nylon 6 include 10 parts of polymethyl methacrylate and 50 parts of nylon 6.

[0033] Example 7 The difference between this embodiment and embodiment 6 is that, in this embodiment, the raw materials of modified nylon 6 include 6 parts of polyurethane elastomer, 4 parts of polymethyl methacrylate and 50 parts of nylon 6; The preparation method of modified nylon 6 comprises the following steps: 4 parts of polymethyl methacrylate and 6 parts of polyurethane elastomer are blended and melted at 175°C for 1.5 hours, nylon 6 is added, dispersed evenly, cooled, and granulated to obtain modified nylon 6.

[0034] Example 8 The only difference between this embodiment and embodiment 7 is that in this embodiment, the raw materials of modified nylon 6 include 1 part of polyurethane elastomer, 9 parts of polymethyl methacrylate and 50 parts of nylon 6.

[0035] Example 9 The only difference between this embodiment and embodiment 7 is that in this embodiment, the raw materials of modified nylon 6 include 5 parts of polyurethane elastomer, 5 parts of polymethyl methacrylate and 50 parts of nylon 6.

[0036] Example 10 The only difference between this embodiment and embodiment 7 is that in this embodiment, the raw materials of modified nylon 6 include 2 parts of polyurethane elastomer, 8 parts of polymethyl methacrylate and 50 parts of nylon 6.

[0037] Embodiment 11 The only difference between this embodiment and Embodiment 10 is that in this embodiment, the rectorite is modified rectorite, and the raw materials of the modified rectorite include 15 parts of rectorite and 5 parts of dioctadecyl dimethyl ammonium chloride; the preparation method of the modified rectorite includes the following steps: dissolving 5 parts of dioctadecyl dimethyl ammonium chloride in ethanol to obtain a mixed solution with a mass fraction of 18%, adding 15 parts of rectorite to the mixed solution with a mass fraction of 18%, stirring until the rectorite is evenly dispersed, concentrating, and drying to obtain the modified rectorite.

[0038] Example 12 The only difference between this embodiment and Embodiment 10 is that in this embodiment, the rectorite is modified rectorite, and the raw materials of the modified rectorite include 15 parts of rectorite and 5 parts of potassium oleate; the preparation method of the modified rectorite includes the following steps: dissolving 5 parts of potassium oleate in ethanol to obtain a mixed solution with a mass fraction of 18%, adding 15 parts of rectorite to the mixed solution with a mass fraction of 18%, stirring until the rectorite is evenly dispersed, concentrating, and drying to obtain the modified rectorite.

[0039] Embodiment 13 The only difference between this embodiment and Embodiment 10 is that in this embodiment, the rectorite is modified rectorite, and the raw materials of the modified rectorite include 15 parts of rectorite, 2.5 parts of potassium oleate and 2.5 parts of dioctadecyl dimethyl ammonium chloride; the preparation method of the modified rectorite includes the following steps: dissolving 2.5 parts of potassium oleate and 2.5 parts of dioctadecyl dimethyl ammonium chloride in ethanol to obtain a mixed solution with a mass fraction of 18%, adding 15 parts of rectorite to the mixed solution with a mass fraction of 18%, stirring until the rectorite is evenly dispersed, concentrating, and drying to obtain the modified rectorite.

[0040] Embodiment 14 The only difference between this embodiment and Embodiment 13 is that, in this embodiment, the raw materials of the modified rectorite include 19 parts of rectorite, 0.5 parts of potassium oleate and 0.5 parts of dioctadecyl dimethyl ammonium chloride.

[0041] Embodiment 15 The only difference between this embodiment and Embodiment 13 is that, in this embodiment, the raw materials of the modified rectorite include 18 parts of rectorite, 1 part of potassium oleate and 1 part of dioctadecyl dimethyl ammonium chloride.

[0042] Example 16 The only difference between this embodiment and embodiment 13 is that in this embodiment, the raw materials of the modified rectorite include 16 parts of rectorite, 2 parts of potassium oleate and 2 parts of dioctadecyl dimethyl ammonium chloride.

[0043] Comparative Example 1 The only difference between this comparative example and Example 1 is that in this comparative example, 50 parts of modified nylon 6 are replaced by an equal amount of nylon 6.

[0044] Comparative Example 2 The only difference between this comparative example and Example 1 is that in this comparative example, no rectorite is added.

[0045] The engineering plastics for communication optical cables prepared in Examples 1 to 16 and Comparative Examples 1 to 2 were subjected to the following performance tests: ① Tensile properties: The tensile strength of engineering plastics used for communication optical cables was tested according to the test method in GB / T 1040.1-2018 "Determination of tensile properties of plastics Part 1: General Principles", where the test speed was 100 mm / min; the test result was the average value of 5 samples; ② Wear resistance: According to the test method in GB / T 3960-2016 "Plastic Sliding Friction Wear Test Method", the wear amount of engineering plastics used for communication optical cables is tested; the test speed is 200r / min, the test time is 2h, the load is 40kg, and the test result is the average value of 3 samples; The test results are shown in Table 1 below: Table 1 Performance test results of Examples 1 to 16 and Comparative Examples 1 to 2

[0046] Compared with Comparative Example 1, the tensile strength of Example 1 is significantly improved, and the wear amount is significantly reduced, indicating that the use of polymethyl methacrylate to mix and modify nylon 6 can improve the wear resistance and tensile properties of engineering plastics used for communication optical cables. Compared with Comparative Example 2, the tensile strength of Example 1 is significantly improved, and the wear amount is significantly reduced, indicating that the addition of rectorite can also improve the wear resistance and tensile properties of engineering plastics used for communication optical cables.

[0047] Compared with Examples 2 and 4, the tensile strength of Examples 5-6 is improved and the wear amount is reduced, indicating that when the weight ratio of nylon 6 to polymethyl methacrylate is 5-9:1, the wear resistance and tensile properties of the engineering plastics used for communication optical cables can be further improved.

[0048] Compared with Example 6, the wear amount of Examples 7 to 10 is reduced, indicating that the use of polyurethane elastomer and polymethyl methacrylate to modify nylon 6 can further improve the wear resistance of engineering plastics used for communication optical cables. Compared with Examples 7 to 8, the wear amount of Examples 9 to 10 is reduced, indicating that when the weight ratio of nylon 6, polymethyl methacrylate and polyurethane elastomer is 50:5 to 8:2 to 5, the use of polyurethane elastomer and polymethyl methacrylate to modify nylon 6 can further improve the wear resistance of engineering plastics used for communication optical cables.

[0049] Compared with Examples 10 to 12, the wear amount of Examples 13 to 16 is reduced, indicating that the surface modification of rectorite using potassium oleate and dioctadecyl dimethyl ammonium chloride can further improve the wear resistance of engineering plastics used for communication optical cables. In addition, compared with Examples 13 to 14, the wear amount of Examples 15 to 16 is reduced, indicating that when the weight ratio of rectorite, potassium oleate and dioctadecyl dimethyl ammonium chloride is 8 to 18:1:1, the wear resistance of engineering plastics used for communication optical cables can be further improved.

[0050] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An engineering plastic for communication optical cable, characterized in that: The composition comprises the following components in parts by weight: 50-70 parts of modified nylon 6, 10-15 parts of polyethylene terephthalate, 15-25 parts of rectorite, 1-5 parts of compatibilizer, 1-3 parts of antioxidant, 0.5-1.5 parts of lubricant; The raw materials of the modified nylon 6 include polymethyl methacrylate and nylon 6.

2. The engineering plastic for communication optical cable according to claim 1, characterized in that: The weight ratio of the nylon 6 to the polymethyl methacrylate is 5-9:

1.

3. The engineering plastic for communication optical cable according to claim 1, characterized in that: The preparation method of the modified nylon 6 comprises the following steps: melting the polymethyl methacrylate, adding nylon 6, blending, cooling, and granulating to obtain the modified nylon 6.

4. The engineering plastic for communication optical cable according to claim 1, characterized in that: The raw materials of the modified nylon 6 also include polyurethane elastomer.

5. The engineering plastic for communication optical cable according to claim 4, characterized in that: The weight ratio of nylon 6, polymethyl methacrylate and polyurethane elastomer is 50:5-8:2-5.

6. The engineering plastic for communication optical cable according to claim 1, characterized in that: The rectorite is modified rectorite, and the raw materials of the modified rectorite include rectorite, potassium oleate and dioctadecyl dimethyl ammonium chloride.

7. The engineering plastic for communication optical cable according to claim 6, characterized in that: The preparation method of the modified rectorite comprises the following steps: dissolving the potassium oleate and the dioctadecyl dimethyl ammonium chloride in ethanol to obtain a mixed solution, adding the rectorite to the mixed solution, dispersing evenly, concentrating, and drying to obtain the modified rectorite.

8. The engineering plastic for communication optical cable according to claim 6, characterized in that: The weight ratio of the rectorite, potassium oleate and dioctadecyl dimethyl ammonium chloride is 8-18:1:

1.

9. The engineering plastic for communication optical cable according to claim 1, characterized in that: The compatibilizer is one or more of maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, and maleic anhydride grafted ethylene-vinyl acetate copolymer; the antioxidant is one or more of antioxidant 1010, antioxidant 168, and antioxidant 1076; and the lubricant is one or both of polyethylene wax and calcium stearate.

10. A method for preparing engineering plastics for communication optical cables according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: blending the components in parts by weight, extruding and granulating, and obtaining engineering plastics for communication optical cables.

Citation Information

Patent Citations

  • Glass fiber reinforced nylon 6-polyethylene terephthalate alloy material and preparation method thereof

    CN102558844A

  • Thermoplastic resin composition

    JP1994340801A

  • Polyester / polyamide resin compositions containing grafted polyolefin and molded products thereof

    US4879341A

  • Process for producing reinforced crystalline engineering plastic composition

    US5367013A

  • Molded article of fiber-reinforced thermoplastic resin, process for producing the same, and long-fiber-reinforced thermoplastic resin composite

    US5866256A