Flexible self-adhesion super-hydrophobic photo-thermal deicing film and preparation method thereof
Through flexible self-adhesive superhydrophobic photothermal ice removal film, graphene oxide and acidified spiral carbon nanotube combined with plasma treatment, the problems of low efficiency and easy material damage are solved, and high efficiency is achieved. Economical and environmentally friendly deicing effect, and improves the adhesion and thermal conductivity of the film.
Patent Information
- Application Number
- CN202411158667.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional deicing methods are low-efficiency, high energy consumption, high cost and chemically contaminated. Superhydrophobic materials are easily damaged in extreme environments and cannot meet the anti-icing needs.
Using flexible self-adhesive superhydrophobic photothermal deicing film, the self-cleaning, water evaporation and deicing functions are achieved through synergistic photothermal effect, graphene oxide and acidified spiral carbon nanotube combination materials are used to improve the self-adhesion of the film. It also has superhydrophobic properties.
It realizes an efficient, economical and environmentally friendly icing solution. The film can completely deicate it in a short time and improves adhesion and thermal conductivity. It is suitable for material surfaces of different shapes.
Smart Images

Figure CN119039938A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a flexible self-adhesive super-hydrophobic photothermal deicing film and a preparation method thereof, belonging to the technical field of functional materials and preparation thereof. Background Art
[0002] As a natural phenomenon, ice's unique shape and structure give it extremely high aesthetic value. However, ice formation or accumulation on surfaces such as aircraft wings and engine air intakes, power transmission lines, and high-speed train bogies may have catastrophic effects on various systems. Therefore, anti-icing and rapid de-icing technologies are crucial.
[0003] Traditional deicing methods such as anti-icing fluid, mechanical deicing and heating deicing (electric heating, hot air) often involve complex preparation routes, or are accompanied by low efficiency, energy consumption, high cost and chemical pollution. Superhydrophobic interface is considered to be one of the most promising anti-icing technologies, with the advantages of no energy consumption, low adhesion, and effective delay of ice crystal growth. The surface of superhydrophobic material is composed of micro-nanoscale rough structure, which is easily damaged by external impact or low temperature and high humidity environment, thus affecting its superhydrophobic performance. In extreme environments, superhydrophobic materials cannot meet the anti-icing needs. Summary of the invention
[0004] In view of the above technical problems existing in the existing deicing methods, the present invention provides a flexible self-adhesive super-hydrophobic photothermal deicing film and a preparation method thereof. Specifically, the surface of the super-hydrophobic film using the synergistic photothermal effect has the functions of self-cleaning, water evaporation and deicing, which solves the icing problem more efficiently, economically and environmentally friendly. At the same time, the self-adhesive properties of the film are utilized, and it can be firmly bonded to materials of different shapes without additional fasteners, reducing the complexity of the system, and having the characteristics of flexible application and easy implementation.
[0005] The technical solution of the present invention:
[0006] One of the purposes of the present invention is to provide a method for preparing a flexible self-adhesive super-hydrophobic photothermal deicing film, the method comprising the following steps:
[0007] (1) Using graphene oxide (GO) aqueous solution and acidified helical carbon nanotubes (HCNTs) aqueous solution as raw materials, reacting in a water bath in the presence of a reducing agent to obtain HCNTs-rGO;
[0008] (2) mixing styrene-ethylene-butadiene-styrene block copolymer (SEBS), toluene and HCNTs-rGO, heating and stirring to obtain an organic suspension;
[0009] (3) pouring the organic suspension into a mold and heating to volatilize toluene to obtain a flexible film;
[0010] (4) protecting one side of the flexible film with aluminum foil and treating the other side with oxygen plasma to obtain a self-adhesive flexible film;
[0011] (5) Aluminum foil was used to protect the surface of the self-adhesive flexible film, and the other side was treated with tetrafluoromethane plasma to obtain a flexible self-adhesive superhydrophobic photothermal deicing film.
[0012] It is further defined that the reducing agent in (1) is an aqueous solution of tea polyphenols.
[0013] It is further defined that the preparation method of the acidified helical carbon nanotubes in (1) is as follows: the helical carbon nanotubes are mixed with concentrated nitric acid, kept at a constant temperature of 160° C. in a forced air drying oven for 6 to 8 hours, cooled to room temperature, and then rinsed with ethanol and deionized water until neutral to obtain the acidified helical carbon nanotubes.
[0014] It is further defined that the water bath reaction temperature in (1) is 80-90° C., the reaction time is 8-12 h, and the stirring rate is 400-600 r / min.
[0015] Further defined, the specific operation process of (1) is: take 10mL of 3mg / mL graphene oxide aqueous solution and ultrasonicate it for 2h, mix it with 20mL of 0.5mg / mL acidified spiral carbon nanotube aqueous solution and ultrasonicate it for 1.5h, then add 30mL of 10mg / mL tea polyphenol aqueous solution, and mechanically stir it at 400-600r / min in a constant temperature water bath at 80-90℃ for 8-12h.
[0016] Further defined, the preparation method of graphene oxide aqueous solution is: 16.1mL concentrated sulfuric acid and 0.7g natural flake graphite powder are placed in an ice water bath at -1 to 1°C and stirred for 0.5 to 1h, and then 4.2g potassium permanganate (KMnO4) is added in batches, and after the addition of KMnO4 is completed, the stirring is continued in the ice water bath for 2.5 to 3h, and the stirring speed is 600 to 800r / min; then placed in a constant temperature water bath at 40 to 45°C, mechanically stirred for 20 to 30min, and a reddish brown viscous liquid is obtained, and the temperature is continued to rise to 80 to 85°C, 49mL deionized water is added in batches, and after stirring for 20min, 42mL deionized water is added; 7mL 30% hydrogen peroxide was diluted with 35 mL of deionized water and then added to the above mixture. The solution immediately turned golden yellow. The obtained solution was filtered and washed with 45 mL of 3.7 wt% hydrochloric acid for 12 h. After filtering again, the filter cake was dispersed in deionized water and stirred at a speed of 600-800 r / min for 12 h. The solution was then centrifuged at 3500 rpm for 30-40 min to remove unpeeled graphite. The supernatant was retained and poured into a dialysis bag. Dialysis was performed for one week to remove residual ions to obtain an aqueous solution of graphene oxide.
[0017] It is further defined that the molecular weight cut-off of the dialysis bag is 8000 to 14000 Da.
[0018] It is further defined that (2) in the obtained organic suspension, HCNTs-rGO accounts for 5-30% of the total mass of HCNTs-rGO and SEBS, and the volume ratio of SEBS mass to toluene is 1 g: (3-20) mL.
[0019] It is further defined that in (2), after SEBS and toluene are mixed, the heating and stirring temperature is 50-70°C for 4-6 hours; after HCNTs-rGO is added, the heating and stirring temperature is 40-60°C for 6-8 hours.
[0020] It is further defined that the temperature for heating and volatilizing toluene in (3) is 40 to 50°C.
[0021] It is further defined that the oxygen plasma treatment power in (4) is 50 to 200 W and the treatment time is 10 to 30 s.
[0022] It is further defined that the tetrafluoromethane plasma treatment in (5) has a power of 50 to 200 W and a treatment time of 1 to 3 minutes.
[0023] The second object of the present invention is to provide a flexible self-adhesive super-hydrophobic photothermal deicing film obtained by the above-mentioned preparation method.
[0024] It is further defined that the film thickness is 10 to 200 μm.
[0025] Beneficial effects:
[0026] The present invention first constructs a spiral carbon nanotube-graphene three-dimensional structure, and uses spiral carbon nanotubes to support the graphene layer structure, thereby reducing the reduction in thermal conductivity caused by graphene stacking and carbon nanotube agglomeration, and improving the overall thermal conductivity of the composite material. The experimental results show that under the illumination of one sun, the composite structure film can increase the temperature to above 69°C within 270s at room temperature. At the same time, the film is placed on a -30°C cold plate with a relative humidity of 70±5%, and the 3mm thick ice layer on the surface can be melted and removed within 16 minutes, maintaining the surface temperature at about 18°C.
[0027] In addition, the present invention treats the surface of the flexible film by oxygen plasma, and utilizes the active components in the plasma to recombine with the chemical bonds broken by electron bombardment on the surface, which remain on the surface to activate the surface and improve the self-adhesive film adhesion. Compared with the surface of the flexible film that has not been treated with plasma, the adhesion is increased by 60 to 140%. Further, by treating another layer of the surface of the flexible film with tetrafluoromethane plasma, the inherent roughness of the surface can be reduced to achieve surface super-hydrophobicity, which can reduce the probability of icing, the area of icing and the strength of ice adhesion. The light and heat work together with the super-hydrophobicity to achieve complete de-icing of the material surface in a short time. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 These are photos of the film prepared in Example 2 adhered to a glass surface, a cylindrical high-density polyethylene surface, and an aluminum surface, wherein a is adhered to a glass surface, b is adhered to a cylindrical high-density polyethylene surface, and c is adhered to an aluminum surface;
[0029] Figure 2 is the contact angle between the film prepared in Example 2 and water;
[0030] Figure 3 The contact angle between the film surface and water prepared in Comparative Example 1;
[0031] Figure 4 The tensile test results of the film prepared in Example 2 are as follows;
[0032] Figure 5 The interfacial adhesion test results of the films prepared in Examples 1 to 3 and Comparative Example 1 are shown;
[0033] Figure 6 The temperature rise curves of the films prepared in Example 2 and Comparative Examples 2-3 under 1 sun illumination;
[0034] Figure 7 This is the actual effect diagram of ice layer changes during the thin film deicing process prepared in Example 2 and the corresponding infrared thermal imaging diagram. DETAILED DESCRIPTION
[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0036] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0037] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0038] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained by those skilled in the art through commercial channels, and the purity of the solid and liquid reagents used is analytically pure.
[0039] Example 1
[0040] The method for preparing a flexible self-adhesive super-hydrophobic photothermal deicing film in this embodiment is carried out according to the following steps:
[0041] Step 1: Preparation of HCNTs-rGO
[0042] (1) Preparation of acidified helical carbon nanotube aqueous solution:
[0043] 0.3 g HCNTs (purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.) and 3 mL of 68% concentrated nitric acid were placed in a 50 mL autoclave and kept at 160°C in a forced air drying oven for 8 h. After cooling to room temperature, the acidified HCNTs were rinsed with ethanol and deionized water for 6 times until neutralized, and then prepared with deionized water to a concentration of 0.5 mg / mL for storage.
[0044] (2) Preparation of graphene oxide aqueous solution:
[0045] Place 16.1 mL of 98% concentrated sulfuric acid and 0.7 g of natural flake graphite powder in a 0°C ice-water bath and stir for 1 h. Then add a total of 4.2 g of KMnO4 in 10 batches. After all the KMnO4 has been added, continue stirring in the ice-water bath for 2.5 h at a stirring speed of 800 r / min. Then place in a 40°C constant temperature water bath and mechanically stir for 20 min to obtain a reddish-brown viscous liquid. Continue to heat to 80°C, add a total of 49 mL of deionized water in 20 batches, stir for 20 min, and then add 42 mL of deionized water. 7 mL of 30% hydrogen peroxide was diluted with 35 mL of deionized water and then added to the above mixture. The solution immediately turned golden yellow. The obtained solution was filtered and washed with 45 mL of 3.7 wt% hydrochloric acid for 12 h. After filtering again, the filter cake was dispersed in deionized water and stirred at 800 r / min for 12 h. The solution was then centrifuged at 3500 rpm for 40 min to remove unpeeled graphite. The supernatant was retained and poured into a dialysis bag (molecular weight cutoff of 8000-14000 Da). It was dialyzed for one week to remove residual ions to obtain graphene oxide. The concentration was diluted to 3 mg / mL with deionized water to obtain a graphene oxide aqueous solution.
[0046] (3) Preparation of HCNTs-rGO:
[0047] Take 10 mL of 3 mg / mL graphene oxide aqueous solution and ultrasonicate it for 2 h, mix it with 20 mL of 0.5 mg / mL acidified spiral carbon nanotube aqueous solution and ultrasonicate it for 1.5 h, then add 30 mL of 10 mg / mL tea polyphenol aqueous solution, and mechanically stir it in a constant temperature water bath at 90°C and 400 r / min for 8 h. After the reaction, wash it with deionized water to obtain HCNTs-rGO.
[0048] Step 2: Preparation of flexible film
[0049] SEBS was mixed with toluene, heated to 70°C and stirred for 6 hours until uniformly stirred, HCNTs-rGO was added, heated to 50°C and stirred for 8 hours to obtain an organic suspension; the organic suspension was poured into a polytetrafluoroethylene mold (mold size was 4 cm×4 cm×1 mm), the organic solvent was evaporated at 40°C, and a flexible film with a thickness of 50 μm was obtained.
[0050] The mass ratio of HCNTs-rGO to SEBS in the organic suspension was 1:5, and the volume ratio of SEBS mass to toluene was 1 g:6.6 mL.
[0051] Step 3: Self-adhesion and super-hydrophobic treatment
[0052] The flexible film obtained in step 2 was protected on one side with aluminum foil, and the other side was treated with oxygen plasma for 10 seconds at a treatment power of 100 W to obtain a self-adhesive flexible film. The surface of the self-adhesive flexible film was protected with aluminum foil, and the other side was treated with tetrafluoromethane plasma for 90 seconds at a treatment power of 100 W to obtain a flexible self-adhesive super-hydrophobic photothermal deicing film.
[0053] Example 2
[0054] The difference between this embodiment and embodiment 1 is that in step 3, oxygen plasma treatment is performed for 20 seconds with a treatment power of 150 W, and the remaining process steps and parameter settings are the same as those in embodiment 1.
[0055] Example 3
[0056] The difference between this embodiment and embodiment 1 is that the mass ratio of HCNTs-rGO to SEBS in the organic suspension in step 2 is 1:3, and the remaining process steps and parameter settings are the same as those in embodiment 1.
[0057] Comparative Example 1
[0058] The difference between this embodiment and embodiment 1 is that step 3 is not performed, and the remaining process steps and parameter settings are the same as those in embodiment 1.
[0059] Comparative Example 2
[0060] The difference between this embodiment and embodiment 1 is that HCNTs are used instead of HCNTs-rGO in step 2, and the remaining process steps and parameter settings are the same as those in embodiment 2.
[0061] Comparative Example 3
[0062] The difference between this embodiment and embodiment 1 is that graphene is used instead of HCNTs-rGO in step 2, and the remaining process steps and parameter settings are the same as those in embodiment 2.
[0063] Effect example
[0064] (1) The adhesion of the flexible self-adhesive super-hydrophobic photothermal deicing film prepared in Example 2 was tested. Figure 1 Figures a, b and c are photos of the flexible self-adhesive super-hydrophobic photothermal deicing film prepared in Example 2 adhered to a glass surface, a cylindrical high-density polyethylene surface and an aluminum surface, respectively. Figure 1 It can be seen that the film prepared in Example 2 has flexibility and self-adhesion.
[0065] (2) The contact angles of the flexible self-adhesive super-hydrophobic photothermal deicing film prepared in Example 2 and the contact angles of the film prepared in Comparative Example 1 with water are as follows: Figure 2 and Figure 3 As shown. Figure 2 and Figure 3 It can be seen that the film prepared in Example 2 has super-hydrophobicity, while the film prepared in Comparative Example 1 does not have super-hydrophobicity, which indicates that the tetrafluoromethane plasma treatment makes the film super-hydrophobic.
[0066] (3) The mechanical properties of the flexible self-adhesive super-hydrophobic photothermal deicing film prepared in Example 2 were characterized. The results of the tensile test (experimental rate was 5 mm / min) were as follows: Figure 4 As shown, the experimental results show that the elongation at break of the film reaches 420%, and the film exhibits excellent tensile properties.
[0067] (4) Test the interfacial adhesion according to the standard 90° peel test method. Figure 5 The test results of the adhesion of the films prepared in Examples 1 to 3 and Comparative Example 1 on glass are shown in FIG. Figure 5 It can be seen that the adhesion of the film prepared in Example 2 on the glass is 18.5 N / cm, which is 140% higher than that of Comparative Example 1.
[0068] (5) The photothermal properties of the films prepared in Example 2, Comparative Example 2 and Comparative Example 3 were tested. The temperature rise curves under 1 sun illumination were as follows: Figure 6 As shown, curve a corresponds to Example 2, curve b corresponds to Example 2, and curve c corresponds to Example 3. Figure 6It can be seen that the film prepared in Example 2 has an excellent photothermal performance when the temperature rises to 69.5° C. within 270 seconds at room temperature under 1 sun illumination.
[0069] (6) The film prepared in Example 2 was subjected to a deicing experiment. Specifically, a 3 mm ice layer was frozen on the surface of a 5 cm × 5 cm film. The film was placed on a cold plate at -30°C and a relative humidity of 70 ± 5%. -2 After 16 minutes of irradiation under strong light, the film can completely melt the surface ice and remove it, and the surface temperature finally rises to about 18°C. The actual effect of the ice layer change during the test and the corresponding infrared thermal imaging are shown in the figure below. Figure 7 shown.
[0070] Although the present invention has been disclosed as above in the preferred embodiments, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing a flexible self-adhesive super-hydrophobic photothermal deicing film, It is characterized in that include: (1) Using graphene oxide aqueous solution and acidified helical carbon nanotube aqueous solution as raw materials, reacting in a water bath in the presence of a reducing agent to obtain HCNTs-rGO; (2) SEBS, toluene and HCNTs-rGO are mixed, heated and stirred to obtain an organic suspension; (3) pouring the organic suspension into a mold and heating to volatilize toluene to obtain a flexible film; (4) protecting one side of the flexible film with aluminum foil and treating the other side with oxygen plasma to obtain a self-adhesive flexible film; (5) Aluminum foil was used to protect the surface of the self-adhesive flexible film, and the other side was treated with tetrafluoromethane plasma to obtain a flexible self-adhesive superhydrophobic photothermal deicing film.
2. The preparation method according to claim 1, It is characterized in that (1) The reducing agent is a tea polyphenol aqueous solution.
3. The preparation method according to claim 1, It is characterized in that (1) The preparation method of neutralized helical carbon nanotubes is as follows: helical carbon nanotubes and concentrated nitric acid are placed in a high-pressure reactor, kept at a constant temperature of 160° C. in a forced air drying oven for 6 to 8 hours, cooled to room temperature, and then rinsed with ethanol and deionized water until neutral, thereby obtaining acidified helical carbon nanotubes.
4. The preparation method according to claim 1, It is characterized in that (1) The reaction temperature in the water bath is 80-90°C, the reaction time is 8-12 hours, and the stirring rate is 400-600 r / min.
5. The preparation method according to claim 1, It is characterized in that (2) In the obtained organic suspension, HCNTs-rGO accounts for 5-30% of the total mass of HCNTs-rGO and SEBS, and the volume ratio of SEBS mass to toluene is 1 g: (3-20) mL.
6. The preparation method according to claim 1, It is characterized in that (2) After SEBS and toluene are mixed, the stirring temperature is heated to 50-70°C for 4-6 hours; after HCNTs-rGO is added, the stirring temperature is heated to 40-60°C for 6-8 hours.
7. The preparation method according to claim 1, It is characterized in that (4) The oxygen plasma treatment power is 50 to 200 W and the treatment time is 10 to 30 seconds.
8. The preparation method according to claim 1, It is characterized in that (5) The tetrafluoromethane plasma treatment power is 50 to 200 W and the time is 1 to 3 minutes.
9. A flexible self-adhesive super-hydrophobic photothermal deicing film obtained by the preparation method according to any one of claims 1 to 8.
10. The flexible self-adhesive super-hydrophobic photothermal deicing film according to claim 9, It is characterized in that The film thickness is 10 to 200 μm.
Citation Information
Cited By
Preparation method and application of super-hydrophobic SiO2 / rGO composite coating
CN120464230A