Method for smelting steel by using straw and forage grass carbon as raw materials instead of coke
By improving the particle size of straw and pasture charcoal and adding combustion aids, the calorific value and combustion performance can be improved, so that it can replace coke in steel smelting, solving the problem of insufficient reduction capacity and achieving low cost, low carbon emissions and high quality Steel production.
Patent Information
- Application Number
- CN202411117139.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, the reduction ability of straw and charcoal is weak and cannot effectively replace coke. During the steel smelting process, it leads to high carbon dioxide emissions and poor steel quality.
By crushing straw and charcoal into 0.15 mm-0.18 mm carbon powder particles, and mixing them with aluminum dihydrogen phosphate inorganic adhesive and dicyclopentadiene iron combustion aid, they are pressed and formed by forming carbon press to improve the Its unit calorific value and combustion properties allow it to replace part or all of coke for steel smelting.
Low-cost and low-carbon emission steel smelting has been achieved, improving the quality and combustion efficiency of steel, reducing slag emissions, and reducing fuel costs.
Abstract
Description
Technical Field
[0001] The invention relates to a steel smelting method, in particular to a steel smelting method using straw and forage charcoal as raw materials to completely or partially replace coke. Background Art
[0002] The process of reducing iron ore with a reducing agent at high temperature to obtain pig iron is called ironmaking. Currently, there are mainly blast furnace method, direct reduction method, molten reduction method, and plasma method. In actual production, pure iron does not exist. The blast furnace smelting method obtains an iron-carbon binary alloy called steel. The main raw materials for ironmaking are iron ore, coke, limestone, and air.
[0003] The reaction formula is:
[0004] Fe2O3+3CO=2Fe+3CO2(high temperature)(reduction reaction)
[0005] Fe3O4+4CO=3Fe+4CO2(high temperature)(reduction reaction)
[0006] Slag formation:
[0007] CaCO3=CaO+CO2(condition: high temperature)
[0008] CaO+SiO2=CaSiO3 (condition: high temperature)
[0009] It can be seen from the above reaction equation that a large amount of carbon dioxide will be released during the iron-making process. In the steel smelting process, carbon dioxide is a by-product that accompanies pig iron and slag.
[0010] It is of particular importance for the steelmaking industry to gradually reduce carbon dioxide emissions per ton of steel and promote energy-saving and carbon-reduction transformation and upgrading in the steelmaking industry in order to meet the challenges of global climate change and achieve sustainable development goals.
[0011] Straw and forage charcoal is a carbon material of agricultural residues. Straw and forage are placed in a sealed container and heated and decomposed under air-tight conditions to make charcoal. Regardless of the production process, charcoal is a product that evaporates the gas and liquid in biomass by heating. The raw materials of charcoal are mainly wood, crop straw, etc. Mechanism-made charcoal is made of biomass fragments as raw materials. The biomass fragments are formed under high temperature and high pressure and sent to the carbonization furnace for carbonization. During the production process, no additives are required, and the manufacturing process is pollution-free. The characteristics of mechanism-made charcoal are long burning time, high calorific value, no smoke, and no pollutant emissions. The main problem of using straw and forage mechanism-made charcoal to replace coke as a raw material for steel smelting is that the reduction ability is weak. For example, charcoal is a porous solid fuel left by pyrolysis of wood or wood raw materials isolated from air. Coke is a solid fuel obtained by pressurizing coal, isolating it from air and distilling it at high temperature. The reducing power of coke is greater than that of charcoal. In addition, charcoal has a large number of micropores and excessive pore structures, and its density is small. Although it has a high specific surface area and good adsorption performance, it is not easy to ignite. The calorific value of combustion per unit volume or mass is low. Summary of the invention
[0012] The purpose of the present invention is to provide a method for smelting steel by using straw and forage charcoal as raw materials instead of coke, which has small carbon emission, good product quality and low cost.
[0013] In order to achieve the above requirements, a technical solution for smelting steel using straw and forage charcoal as raw materials instead of coke is proposed: the characteristic is that during the smelting process, a mixture of coke and straw and forage charcoal is blown into the blast furnace from the bottom; the straw and forage charcoal generates high temperature during the combustion process, and the iron ore is heated to a sufficiently high temperature to melt the iron ore; CO gas is generated during the combustion of the straw and forage charcoal, and metal oxides are reduced to metals through the reaction; the straw and forage charcoal itself is composed of carbon elements, and during the smelting process, it provides a reducing agent to accelerate the degradation and decomposition of metals; since the commonly used straw and forage charcoal has a calorific value per unit volume or per unit mass, CO gas is generated during the combustion process, and metal oxides are reduced to metals through the reaction; the straw and forage charcoal itself is composed of carbon elements, and during the smelting process, it provides a reducing agent to accelerate the degradation and decomposition of metals; Lower than coke, the straw and forage shaped charcoal used in this steel smelting is made by processing straw and forage into charcoal, and then crushing the charcoal into carbon powder particles with a particle size diameter of 0.15 mm - 0.18 mm. The carbon powder particles are mixed with inorganic adhesives and combustion aids to form a mixture, and the mixture is sent to a forming charcoal press. The forming charcoal press adopts a pressurized method to obtain block or granular straw and forage shaped charcoal materials with a unit calorific value close to or the same as that of coke. Since commonly used straw and forage charcoal is not easy to ignite, a combustion aid is added to the mixture when pressing the shaped charcoal to reduce the ignition point of the shaped charcoal and granular charcoal, so that the obtained straw and forage shaped charcoal can be quickly ignited.
[0014] The inorganic adhesive is aluminum dihydrogen phosphate.
[0015] The combustion improver is dicyclopentadiene iron.
[0016] In the mixed material, the carbon powder particles account for 95%-93% of the total weight, the inorganic adhesive accounts for 5%-3% of the weight, and the combustion aid accounts for 3%-2% of the weight.
[0017] The specific gravity of the formed carbon is 1.4-1.6 g / cm3.
[0018] When smelting steel, the ratio of forming carbon to coke is 100:0-10:90.
[0019] According to the above scheme, a method for smelting steel using straw and forage charcoal as raw materials to replace coke is designed. Without changing the blast furnace smelting process, straw and forage shaped charcoal is used to replace part or all of the coke. Since the shaped charcoal material is made of straw and forage charcoal as the main raw materials, adhesives and combustion aids are added after crushing and then pressurized by a press, the calorific value per unit volume or per unit mass of the straw and forage charcoal is increased by the addition of adhesives and the pressurization of the press, making it equivalent to that of coke. At the same time, the addition of combustion aids lowers the ignition point of the shaped charcoal and granular charcoal and makes it easy to stick together and form when pressurized, so that the prepared straw and forage charcoal can be quickly ignited and can be easier to ignite than coke. Due to such improvements on straw and forage charcoal, straw and forage charcoal can replace coke in the smelting of steel. Straw and forage shaped charcoal has the advantages of long combustion time, high calorific value, no smoke and no explosion. At the same time, straw and forage shaped charcoal does not contain sulfur, no sulfide emissions during combustion, less ash and less slag emissions after straw and forage shaped charcoal combustion. In addition, because straw and forage shaped charcoal replaces coke, it reduces harmful elements in coke and improves the quality of steel. DETAILED DESCRIPTION
[0020] The present invention will be further described below by way of examples.
[0021] A method for smelting steel by using straw and forage charcoal as raw materials to replace coke. During the smelting process, a mixture of coke and straw and forage charcoal is blown into the bottom of a blast furnace. The straw and forage charcoal generates high temperature during combustion, and heats iron ore to a sufficiently high temperature to melt the iron ore. CO gas (carbon monoxide) is generated during the combustion of the straw and forage charcoal, and metal oxides are reduced to metals through reaction. The straw and forage charcoal itself is composed of carbon elements, and during the smelting process, it provides a reducing agent to accelerate the degradation and decomposition of metals. Since the calorific value per unit volume or per unit mass of commonly used straw and forage charcoal is lower than that of coke, the straw and forage charcoal used in the steel smelting process has a lower calorific value than coke. After the straw and forage are processed into charcoal, the charcoal is crushed into carbon powder particles with a particle size of 0.15 mm to 0.18 mm, and the carbon powder particles are mixed with an inorganic adhesive of aluminum dihydrogen phosphate and a combustion aid of dicyclopentadiene iron to make a mixture, in which the carbon powder particles account for 95% to 93% of the total weight, the inorganic adhesive accounts for 5% to 3% of the weight, and the combustion aid accounts for 3% to 2% of the weight. The mixture is sent to a forming charcoal press, and the forming charcoal press adopts a pressurized method to obtain a block or granular straw and forage (biomass) forming charcoal material with a unit calorific value close to or the same as that of coke, and the specific gravity of the forming charcoal is 1.4 to 1.6 g / cubic centimeter. Since the commonly used straw and forage charcoal is not easy to ignite, when pressing the forming charcoal, the combustion aid is mixed into the mixture to reduce the ignition point of the forming charcoal, so that the obtained straw and forage forming can be quickly ignited. When smelting steel, the ratio of forming carbon material to coke is 100:0-10:90. For example, 80:20, 60:40, 40:60, 20:80, etc. Since the combustion calorific value of straw and forage forming carbon is slightly lower than that of coke, when the proportion of forming carbon added exceeds 50% of coke, the pressure and speed of blowing in the forming carbon need to be increased. The specific values of pressure and speed need to be controlled according to the furnace temperature required by the process in different periods of steel smelting.
[0022] According to the above scheme, a method for smelting steel using straw and forage charcoal as raw materials instead of coke is designed. Under the condition of not changing the blast furnace smelting process, straw and forage shaped charcoal is used to replace part of the coke. Tests with the addition ratios of straw and forage shaped charcoal being 10% and coke 90% and straw and forage shaped charcoal being 20% and coke 80% respectively show that the straw and forage shaped charcoal have the advantages of long burning time, high calorific value, no smoke and no explosion. At the same time, the straw and forage shaped charcoal does not contain sulfur and no sulfide is emitted during combustion. After combustion, the straw and forage shaped charcoal has less ash content and less slag emission.
[0023] Through calculation and test evaluation, the price of straw and forage shaped charcoal is 3150 yuan / ton. When the addition ratio of straw and forage shaped charcoal is 10% and 20%, the cost of a ton of iron fuel is 854.12 yuan and 886.12 yuan respectively. According to the current carbon tax price of 150 yuan / ton of carbon dioxide in my country, the cost of a ton of iron fuel is 847.47 yuan and 872.69 yuan respectively, an increase of 19.35 yuan / ton and 44.57 yuan / ton respectively, with growth rates of 2.34% and 5.38% respectively. The current EU carbon tax price is 100 euros / ton of carbon dioxide, equivalent to more than 700 yuan / ton of carbon dioxide. If calculated according to this carbon tax price, the cost of a ton of iron fuel will not increase, but will decrease.
[0024] Research and practice have shown that both charcoal and coke can be used to smelt pig iron. However, the chemical composition of the smelted pig iron is the same, but its structure and mechanical properties are different. Pig iron smelted with charcoal generally has fine grains, a tight structure, and no cracks. The pig iron smelted with charcoal has a small content of impurities and harmful elements, and is suitable for producing high-quality steel. The composition and structure of straw and forage charcoal are basically the same as those of charcoal.
[0025] The above examples are only preferred embodiments of the present invention, but do not limit the scope of the present invention. All equivalent changes and modifications made within the scope of this application are still within the scope of protection covered by the present invention.
Claims
1. A method for smelting steel using straw and forage charcoal as raw materials instead of coke, Its characteristic is that During the smelting process, a mixture of coke and straw and forage shaped charcoal is blown into the blast furnace from the bottom. The straw and forage shaped charcoal generates high temperature during the combustion process, heating the iron ore to a sufficiently high temperature to melt the iron ore. CO gas is generated during the combustion of the straw and forage shaped charcoal, and the metal oxides are reduced to metals through the reaction. The straw and forage shaped charcoal itself is composed of carbon elements. During the smelting process, it provides a reducing agent to accelerate the degradation and decomposition of metals. Since the calorific value per unit volume or per unit mass of the commonly used straw and forage charcoal is lower than that of coke, the straw and forage shaped charcoal used in this steel smelting is After the straw and forage grass are processed into charcoal, the charcoal is crushed into charcoal powder particles with a particle size of 0.15 mm to 0.18 mm. The charcoal powder particles are mixed with an inorganic adhesive and a combustion aid to form a mixture, which is sent to a forming charcoal press. The forming charcoal press uses a pressurized method to obtain block or granular straw and forage charcoal materials with a unit calorific value close to or the same as that of coke. Since commonly used straw and forage charcoal is not easy to ignite, a combustion aid is added to the mixture when pressing the formed charcoal to reduce the ignition point of the formed charcoal and granular charcoal, so that the obtained straw and forage charcoal can be quickly ignited.
2. A method for smelting steel using straw and forage charcoal as raw materials instead of coke according to claim 1, Its characteristics are The inorganic adhesive is aluminum dihydrogen phosphate.
3. A method for smelting steel using straw and forage charcoal as raw materials instead of coke according to claim 1, Its characteristics are The combustion improver is dicyclopentadiene iron.
4. The method of smelting steel using straw and forage charcoal as raw materials instead of coke according to claim 1, Its characteristics are In the mixed material, the carbon powder particles account for 95%-93% of the total weight, the inorganic adhesive accounts for 5%-3% of the weight, and the combustion aid accounts for 3%-2% of the weight.
5. The method of smelting steel using straw and forage charcoal as raw materials instead of coke according to claim 1, Its characteristics are The specific gravity of the formed carbon is 1.4-1.6 g / cm3.
6. The method of smelting steel using straw and forage charcoal as raw materials instead of coke according to claim 1, Its characteristics are When smelting steel, the ratio of forming carbon to coke is 100:0-10:90.