Raw dolomite converter body fettling process
By preventing slag splashing after tapping, raw dolomite is spread evenly on the iron-facing surface and MgCO3 is decomposed at high temperatures inside the furnace, increasing MgO enrichment. This solves the problems of slag splashing and falling off during the furnace repair process of raw dolomite, achieving furnace lining stability and high-efficiency converter production.
Patent Information
- Application Number
- CN202410975849.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-29
AI Technical Summary
During the process of repairing a furnace with raw dolomite, slag splashing and falling are likely to occur, leading to unstable furnace maintenance and potential safety hazards.
Without slag splashing after tapping, raw dolomite is spread flat on the iron-facing surface. The high temperature inside the furnace decomposes MgCO3, increasing the enrichment of MgO. The supersaturated MgO is sintered on the slag-pouring surface by high-position slag splashing, ensuring that the raw dolomite and slag are viscous and sintered together.
This achieves the goal of preventing slag from splashing or falling, improving the stability of the furnace lining and furnace shape control, and ensuring the high-efficiency and stable production of the converter.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of converter smelting, and in particular to a raw dolomite converter furnace body repairing process. Background Art
[0002] The slag pouring surface of the steelmaking converter body refers to the area on the furnace body surface through which the slag in the converter is discharged during the steelmaking process. This area plays a vital role in the steelmaking process because it is in direct contact with the high-temperature slag in the furnace and needs to withstand extremely high temperatures and erosion by the slag. The slag pouring surface of the steelmaking converter body is severely eroded by chemical erosion, mechanical scouring of scrap steel and erosion of molten iron. Simply using pig iron to fill the slag pouring surface can no longer meet the furnace body maintenance requirements, which poses a hidden danger to the furnace body safety.
[0003] The use of raw dolomite is a common method in the process of converter repair. Raw dolomite contains calcium and magnesium, has a high melting point and is refractory, which makes it an ideal choice for furnace repair materials. In the steelmaking process, dolomite can neutralize acidic slag, increase the basicity of slag, reduce the activity of FeO in slag, and reduce the erosion of slag on the furnace lining. At the same time, raw dolomite is often used as a basic refractory material in furnace repair technology, such as the lining of Martin furnace and Thomas rotary furnace in steelmaking, as well as the bottom and slope materials of basic open-hearth furnaces. Dolomite is also often used as a special charge when smelting high-quality ferromanganese alloys and ferrosilicon alloys. In addition, dolomite can also promote early slag, so that the MgO in the slag reaches a saturated state, so as to improve the viscosity of the slag, have good adhesion to the furnace lining, and play a role in protecting the furnace lining.
[0004] In the prior art, when the raw dolomite supplementation process is applied in converter production, technical problems such as slag splashing and falling are easily generated. Summary of the invention
[0005] Aiming at the technical problems of slag splashing and falling in raw dolomite furnace repairing production, the present invention provides a raw dolomite converter furnace body repairing process, which ensures that the slag after splashing is sticky and does not spray, and ensures that the raw dolomite and the slag are sintered together and do not fall.
[0006] The present invention provides a raw dolomite converter furnace body repairing process, comprising the following steps: S1. After the smelting of the previous furnace is completed, slag is left in the furnace body, and the final slag is prepared to ensure that the final slag is transparent and has good fluidity. When tapping the steel, pay attention to controlling the amount of slag left, and leave as much slag as possible to create conditions for raw dolomite to fill the slag surface; S2. Raw dolomite is placed in the scrap steel bucket, and no slag splashes after the converter body taps out steel; S3, add raw dolomite into the furnace body using a scrap steel bucket, and then spread the raw dolomite flat on the iron surface; S4, slag splashing. After the slag splashing is completed, all the slag is retained for smelting.
[0007] Furthermore, in step S2, the mass of raw dolomite placed in the scrap steel bucket is 1.5-2 t.
[0008] Furthermore, in step S3, raw dolomite is spread on the iron facing surface, and the MgCO3 in the raw dolomite is decomposed by high-temperature melting and cooling in the furnace for 5 minutes to increase the MgO enrichment, and then the slag splashing step in step S4 is performed to better sinter the supersaturated MgO on the slag pouring surface through slag splashing.
[0009] Furthermore, in step S4, the slag splashing adopts high gun position slag splashing, and the material splashing is not allowed, and the slag splashing flow rate is ≤35000m 3 / h, to ensure that the slag after splashing is sticky and that the raw dolomite and slag are sintered together and do not fall off.
[0010] Furthermore, in step S4, the full slag smelting includes pouring the furnace and adding iron after adding scrap steel, and when adding scrap steel, the scrap steel is evenly spread on the slag pouring surface, and when adding iron, the iron is added slowly.
[0011] Furthermore, in step S4, blowing is performed during the full slag smelting process. During the blowing process, the blowing gun position is determined according to the amount of raw dolomite added, which is generally 100-200 mm higher than the normal blowing gun position. The temperature during the blowing process and at the end point is uncontrollably too high to prevent the slag splashing layer from being washed away by high temperature.
[0012] Furthermore, the particle size of raw dolomite is 50-500 mm. Using raw dolomite with large particle size within this range can reduce iron block consumption and reduce production costs.
[0013] Further, the specific steps include: S1. The previous furnace is smelted and slag remains in the furnace body; S2. Raw dolomite is placed in the scrap steel bucket. The mass of raw dolomite placed in the scrap steel bucket is 1.5~2t. No slag splashes after the converter body is tapped. S3, add raw dolomite into the furnace body using a scrap steel bucket, and then spread the raw dolomite flat on the iron surface; Slag splashing is carried out after S4 and 5min. The slag splashing is carried out at a high gun position. Adjustable slag splashing is not allowed. The slag splashing flow rate is ≤35000m3 / h. After the slag splashing is completed, all slag is retained for smelting. The full slag smelting includes pouring the furnace and adding iron after adding scrap steel. When adding scrap steel, the scrap steel should be evenly spread on the slag pouring surface.
[0014] The beneficial effect of the present invention lies in that, in the furnace repairing process provided by the present invention, after the steel is discharged, slag is not splashed first, raw dolomite is put into the furnace body and spread flat on the iron facing surface (large surface of the converter), and high-temperature melting in the furnace is utilized to increase the enrichment of MgO after the raw dolomite is decomposed, and then slag splashing is used to make the supersaturated MgO better sintered on the slag pouring surface, thereby achieving the technical effect of no slag splashing and no falling, which significantly improves the maintenance effect of the furnace lining, effectively ensures the stability of the converter lining, and has good control over the furnace lining furnace shape, thereby ensuring the efficient and stable production of the converter. DETAILED DESCRIPTION
[0015] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0016] Example 1 The present invention provides a raw dolomite converter furnace body repairing process, comprising the following steps: S1. After the smelting of the previous furnace is completed, slag is left in the furnace body, and the final slag is prepared to ensure that the final slag is transparent and has good fluidity. When tapping the steel, pay attention to controlling the amount of slag left, and leave as much slag as possible to create conditions for raw dolomite to fill the slag surface; S2. Raw dolomite is placed in the scrap steel bucket. The mass of raw dolomite placed in the scrap steel bucket is 1.8t, and the particle size range of the raw dolomite placed in the scrap steel bucket is 50-500mm. No slag splashes after the converter body is tapped. S3, add raw dolomite into the furnace body with a scrap steel bucket, and then spread the raw dolomite flat on the iron surface, use the high temperature in the furnace to melt and cool for 5 minutes to decompose the MgCO3 in the raw dolomite, increase the MgO enrichment, and make the supersaturated MgO better sintered on the slag pouring surface by splashing slag; S4, slag splashing, slag splashing adopts high gun position slag splashing, no material splashing, slag splashing flow rate 30000m 3 / h, to ensure that the slag after splashing is sticky, and to ensure that the raw dolomite and slag are sintered together and do not fall off; S5. After the slag splashing is completed, the whole slag smelting is carried out. The whole slag smelting includes pouring the furnace and adding iron after adding scrap steel. When adding scrap steel, the scrap steel should be evenly spread on the slag pouring surface. When adding iron, it should be added slowly. Blowing is carried out during the whole slag smelting process. During the blowing process, the blowing gun position is determined according to the amount of raw dolomite added. It is generally 150mm higher than the normal blowing gun position. The temperature during the blowing process and the terminal point cannot be controlled to be too high to prevent the slag splashing layer from being washed away by high temperature.
[0017] The technical effect achieved by the present invention is that after the steel is discharged, slag is not splashed first, raw dolomite is put into the furnace body and spread on the iron facing surface (large surface of the converter), and the high temperature melting in the furnace is utilized to increase the enrichment of MgO after the raw dolomite is decomposed, and then slag splashing is used to make the supersaturated MgO better sintered on the slag pouring surface, thereby achieving the technical effect of no slag splashing or falling, significantly improving the maintenance effect of the furnace lining, effectively ensuring the stability of the converter lining, and good control of the furnace lining furnace shape, thereby ensuring the efficient and stable production of the converter.
[0018] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.
Claims
1. A raw dolomite converter furnace repair process, characterized in that: The steps include: S1. The previous furnace is smelted and slag remains in the furnace body; S2. Raw dolomite is placed in the scrap steel bucket, and no slag splashes after the converter body taps out steel; S3, add raw dolomite into the furnace body using a scrap steel bucket, and then spread the raw dolomite flat on the iron surface; S4, slag splashing. After the slag splashing is completed, all the slag is retained for smelting.
2. A raw dolomite converter furnace repair process as claimed in claim 1, characterized in that: In step S2, the mass of raw dolomite placed in the scrap steel bucket is 1.5-2 t.
3. A raw dolomite converter furnace repair process as claimed in claim 1, characterized in that: In step S3, the raw dolomite is spread on the iron facing surface for 5 minutes, and then the slag splashing step in step S4 is performed.
4. A raw dolomite converter furnace repair process as claimed in claim 1, characterized in that: In step S4, the slag splashing adopts high gun position slag splashing, and the material splashing is not allowed. The slag splashing flow rate is ≤35000m 3 / h.
5. A raw dolomite converter furnace repair process as claimed in claim 1, characterized in that: In step S4, the full slag smelting includes pouring the furnace and adding iron after adding scrap steel, and when adding scrap steel, the scrap steel is evenly spread on the slag pouring surface.
6. A raw dolomite converter furnace repair process as claimed in claim 1, characterized in that: In step S4, during the full slag smelting process, blowing is performed and the blowing lance position is raised by 100-200 mm.
7. A raw dolomite converter furnace repair process as claimed in any one of claims 1 to 6, characterized in that: The particle size of raw dolomite is 50~500mm.
8. A raw dolomite converter furnace repair process as claimed in any one of claims 1 to 6, characterized in that: The specific steps include: S1, the previous furnace is smelted and slag remains in the furnace body; S2. Raw dolomite is placed in the scrap steel bucket. The mass of raw dolomite placed in the scrap steel bucket is 1.5~2t. No slag splashes after the converter body is tapped. S3, add raw dolomite into the furnace body using a scrap steel bucket, and then spread the raw dolomite flat on the iron surface; Slag splashing after S4 and 5min, the slag splashing adopts high gun position slag splashing, the slag splashing flow rate is ≤35000m 3 / h, after the slag splashing is completed, the slag is retained for smelting. The slag is retained for smelting, which includes pouring the furnace and adding iron after adding scrap steel. When adding scrap steel, the scrap steel should be evenly spread on the slag pouring surface.