Low-cost refining process based on tapping metallurgy and slag metallurgy
By using aluminum-magnesium calcium alloy and premelted refined slag for composite deoxygenation and diffusion deoxygenation in steel metallurgy, the problems of high and unstable aluminum consumption in traditional processes are solved, and low-cost and efficient improvement of molten steel purity and production efficiency are achieved. promote.
Patent Information
- Application Number
- CN202411202663.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing steel industry, the challenge of producing high-quality steel at low cost is to efficiently remove inclusions and oxides from molten steel. The traditional process consumes high and unstable aluminum, making it difficult to meet the demand for rapid production.
Use aluminum-magnesium calcium alloy as composite deoxidant to perform composite deoxidation during the steel discharge process, and after the steel discharge, premelted refined slag is added to deoxidize and create white slag again. Combined with the slag surface, aluminum particles are added directly for diffusion and deoxidation, and adjust the molten steel water. The aluminum content is to improve the purity of the molten steel.
It achieves low cost, low oxidation and efficient removal of inclusions and oxides in molten steel, improves the cleanliness and production efficiency of steel, reduces smelting costs, and simplifies the process flow.
Abstract
Description
Technical Field
[0001] The invention relates to a refining method, in particular to a low-cost refining process based on steelmaking metallurgy and slag metallurgy. Background Art
[0002] At present, electric furnace and converter steelmaking generally adopt off-furnace refining technology, that is, all or part of the deoxidation, desulfurization, gas reduction, inclusion reduction, adjustment of steel composition and temperature in the steelmaking process are transferred to the refining process to obtain clean steel and achieve good results of high yield and high quality. However, with the continuous expansion of the international economic crisis and customers' high-quality requirements for steel, low-cost production of high-quality steel has become a development trend in the domestic and foreign steel industry. Due to the consumption of a large amount of materials and human resources by LF refining processes, the cost is relatively high, especially with the continuous application of high-efficiency continuous casting machines, relying on LF refining to produce high-cleanliness molten steel can no longer meet the rapid production needs of steel mills.
[0003] Some steel mills at home and abroad also have a post-steel argon blowing refining process for aluminum-deoxidized killed steel. They all add sufficient aluminum strong deoxidizers and slag-making agents such as pre-melted slag and lime during the steel-making process, use the aluminum-killed molten steel that has been deoxidized to strengthen the "slag washing" deoxidation of the high-oxidation converter slag, and melt it with the slag-making material to reform the top slag modification process, and then perform fine-tuning and soft argon blowing at the argon station to directly cast the production method. However, this process requires the removal of some excess oxygen during steel-making, resulting in high aluminum consumption. At the same time, affected by factors such as the amount of slag and the carbon of the final steel-making, the oxygen in the top slag is difficult to remove effectively and is generally high and unstable. In the case of poor argon blowing and slag removal in individual furnaces, long-term continuous casting and other conditions, a certain depth of flocculent inclusions and a viscous layer that is difficult to float up are likely to form under the top slag, which is likely to cause the flocculent flow of the large ladle in the later stage to fail to keep up with the pouring speed of the middle ladle, and forced production problems such as oxygen burning, rod punching, and speed reduction, which have an adverse effect on quality control. Moreover, this process generally requires matching calcium treatment modification operations to ensure the purity and castability of the molten steel. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a low-cost refining process based on steelmaking metallurgy and slag metallurgy, which can effectively improve the purity of molten steel.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention includes the following process steps: (1) adding aluminum-magnesium-calcium alloy as a composite deoxidizer to the ladle for composite deoxidation during steel tapping;
[0006] (2) Steels with nitrogen requirements below 30 ppm are tapped using non-deoxidation or semi-deoxidation processes, while other steels are tapped using full deoxidation processes; pre-melted refined slag is added after tapping for re-deoxidation and white slag production;
[0007] (3) After steel is tapped, the [Als] content in the steel is controlled to be 0.005-0.020%. After entering the argon station, aluminum particles are added to the slag surface for slag surface deoxidation and aluminum adjustment. During the process, the [Als] content in the molten steel is always maintained at ≥ 0.02%.
[0008] Furthermore, in the step (1), after tapping, the ladle top slag C / A is maintained at 1.7 to 2.0 and MI is maintained at 0.25 to 0.40.
[0009] Furthermore, in step (2), the viscosity of the pre-melted refined slag is 1.5-2.0 Pa·s, and the melting point is 1335-1450°C.
[0010] Furthermore, in step (2), for steel produced by a non-deoxidation or semi-deoxidation process, the pre-melted refined slag is a deoxidized pre-melted refined slag, and the addition amount is 1.5-2.5 kg / t steel; for steel produced by a full deoxidation process, the pre-melted refined slag is a deoxidized modified pre-melted refined slag, and the addition amount is 0.5-1.5 kg / t steel.
[0011] Furthermore, in the step (3), during the slag surface deoxidation and aluminum adjustment process, the ladle top slag remains in liquid state, and the C / A ratio is 1.2 to 1.8.
[0012] The beneficial effects of adopting the above technical scheme are as follows: the present invention conducts detailed analysis and experimental research on the adjustment of the steel-making deoxidation slag-making process, the study of the physical properties of the deoxidation slag-making agent mineral phase, the slag sample detection and the optimization of the slag material structure, etc., and utilizes the high oxygen potential of the molten steel from the steel-making to the argon inlet station, adopts a new top slag modification and deoxidation slag-making steel-making metallurgical process that pre-places composite deoxidation and white slag making in the steel-making process, and a subsequent slag metallurgical process of directly adding aluminum particles to the slag surface of the ladle for diffusion deoxidation and aluminum control. Some steel types that had to be treated by LF or RH before now only need to be treated by the "steel-making metallurgy + slag metallurgy" process, which can achieve the effects of deoxidation, desulfurization, and inclusion removal, and improve the fluidity of the ladle slag, replacing the LF and RH refining processes, and coordinating with the fast pace of continuous casting to achieve the purpose of removing inclusions, meet the production requirements of finished molten steel, obtain high-cleanliness steel, and reduce smelting costs.
[0013] The present invention adopts advance deoxidation and slag making in steelmaking metallurgy and diffusion deoxidation and aluminum control in slag metallurgy, which can reduce smelting cost, improve product quality, and improve production efficiency. It has the characteristics of simple equipment and operation, simple and easy process, low production cost and high product quality. DETAILED DESCRIPTION
[0014] This low-cost refining process based on steel-making metallurgy and slag metallurgy is designed to solve two major problems: the difficulty in quickly adsorbing and removing molten steel inclusions under the conditions of fast-paced production and furnace-machine mismatch, and the secondary pollution of molten steel by highly oxidized and unstable top slag oxygen during lifting and steel pouring. First, the strong impact force of molten steel and the high oxygen potential of molten steel in the steel-making process are utilized to pre-place composite deoxidation and white slag making in the steel-making process to form a new top slag modification and slag deoxidation steel-making metallurgical process. Different steel-making metallurgical processes are selected according to different quality requirements of different steel grades, while meeting quality and cost, i.e., efficiency requirements. Subsequently, a new slag metallurgical process is used to directly add aluminum particles to the slag surface of the ladle for diffusion deoxidation and aluminum control, to carry out top slag diffusion deoxidation and adjust the aluminum content in the molten steel, thereby greatly improving the purity of the molten steel. It is especially suitable for aluminum-deoxidized killed steel.
[0015] This refining process adopts the following process steps:
[0016] (1) In the process of steel tapping, aluminum-magnesium-calcium alloy is used to replace aluminum deoxidation alloy for composite deoxidation:
[0017] The aluminum-magnesium-calcium alloy is a molten reduction aluminum-based composite deoxidizing slag-making agent, and its main components are (wt%): Al=10%-45%, CaCO 3 ≤10%、CaF 2 ≤5%, CaO=20%~40%, Al 2 O 3 =20%~40%, MgO=2%~8%, passivated calcium carbide CaC 2 =5%~20%, among which Al 2 O 3 The weight ratio of calcium to CaO is 1:1. After the steel is tapped, it is added to the ladle, and other processes of the existing steel tapping process remain unchanged. Only the aluminum-magnesium-calcium alloy is used to completely replace aluminum for pre-deoxidation. No aluminum deoxidizing alloy such as steel sand aluminum and aluminum blocks is added during steel tapping. The next metallurgical operation is performed according to the oxygen content of the top slag entering the station, the amount of slag, etc., and the amount of other slag materials such as lime is adjusted. After steel tapping, the C / A ratio of the top slag of the ladle is maintained at 1.7-2.0 and MI at 0.25-0.40. The C / A ratio is the calcium-aluminum ratio CaO / Al 2 O 3 MI is the Mannesmann index, MI = CaO / (Al 2 O 3 *SiO 2 ).
[0018] The aluminum-magnesium-calcium alloy can play a role in composite deoxidation and white slag pre-position after being added during the steelmaking process, optimizes the current production process of first removing oxygen from the steel and then removing oxygen from the slag, and improves the purity of molten steel while reducing the non-equilibrium oxygen and aluminum consumption in steelmaking and the secondary aluminum oxide consumption cost of the argon station.
[0019] The composition configuration of the aluminum-magnesium-calcium alloy is as follows: when the aluminum chemical equivalent in the molten steel exceeds the oxygen, the product is Al 2 O 3 Aluminum can reduce the failure tendency and refine the particles, and improve the yield strength and impact toughness of steel. However, pure aluminum has a low density and is easy to float and burn with oxygen in the air, so its utilization rate is low. There are many types of composite deoxidizers, among which the best element combination is Ca and Al. Ca improves the deoxidation ability of Al, and reduces the consumption of aluminum when achieving the same deoxidation effect. At the same time, Al reduces the volatilization loss of Ca (single substance volatilization, composite non-volatility). Adding an appropriate amount of Mg has a large atomic radius, low solubility in molten iron, and a slow melting rate, but a fast reaction rate with oxygen, which is easy to nucleate, promotes the deoxidation of Ca and Al, and reduces the solubility of [Ca] and [Al]. Passivated calcium carbide CaC 2 When used together with aluminum deoxidizer, its purity is not less than 80%, it can replace 50% of its own weight of metal aluminum. The deoxidation products of calcium carbide are CaO and CO. 2 There is no pollution to molten steel. The generated CaO may react with the deoxidation product Al 2 O 3 The formation of low melting point calcium aluminate is conducive to the floating of inclusions. 2 It can stir the molten steel, promote the floating of inclusions, and also has a desulfurization effect on the molten steel.
[0020] The aluminum-magnesium-calcium alloy has a density of less than 3.0 g / cm 3 Since the density of the aluminum-magnesium-calcium alloy is much smaller than that of molten slag and molten steel, it will quickly float to the slag-steel interface after being added during the steel-tapping process during the deoxidation process. The foaming of the top slag caused by the continued carbon-oxygen reaction of high-carbon ferromanganese and the temperature drop of steel-tapping and the decomposition of some carbonates, calcium fluoride and calcium aluminates in the deoxidizer will be used to wrap the high-viscosity foamed slag of the diffusion deoxidizer, blocking the diffusion of oxygen in the molten steel into the slag without hindering the efficient deoxidation effect and slag-making reaction in the slag. After entering the argon station, the aluminum particles on the slag surface will diffuse and deoxidize, and the aluminum oxide will quickly aggregate into large flocculent inclusions and float up with the argon blowing and stirring, increasing the adsorption and inclusion driving force of the low-oxidizing top slag, realizing the composite deoxidation and white slag pre-process of aluminum-deoxidized calm steel, increasing the probability of adsorption and inclusion, and improving the purity of molten steel. At the same time, the calcium in the aluminum-magnesium-calcium alloy can make the deoxidation product form calcium aluminates with a lower melting point, which are easy to float and remove in the molten steel, and can avoid the blockage of the nozzle when pouring molten steel. At the same time, it can significantly reduce the cost of non-equilibrium oxygen and aluminum consumption in steelmaking and secondary aluminum consumption in the argon station.
[0021] (2) After steel is tapped, pre-melted refined slag is added for re-deoxidation and white slag making:
[0022] This method conducts detailed analysis and experimental research on the adjustment of steel-making deoxidation and slag-making process, physical property research of deoxidation slag-making agent mineral phase, slag sample detection and slag material structure optimization, and explores a new steel-making metallurgical process of top slag modification and slag-making deoxidation that utilizes the strong impact force of molten steel and the high oxygen potential characteristics of molten steel in the steel-making process to advance composite deoxidation and white slag to the steel-making process, so as to achieve the purpose of early slag-making, early slagging and early deoxidation, and create preferential conditions for the efficient implementation of subsequent off-furnace refining process.
[0023] According to the principle of similarity, the composition of the pre-melted refined slag added after tapping must be similar to that of the inclusions in the molten steel. To ensure good fluidity of the refined slag, the viscosity of the refined slag is controlled at 1.5-2.0 Pa·s and the melting point is controlled at 1335-1450℃. The amount of pre-melted refined slag added is adjusted according to the (FeO) content in the converter terminal slag and the amount of slag in the tapping belt. All pre-melted refined slag is added to the ladle after tapping.
[0024] The following deoxidized premelted refined slag and deoxidized modified premelted refined slag are two types of premelted refined slag, with slightly different compositions and functions. The main function of the deoxidized premelted refined slag is deoxidation, and the content of deoxidizers such as aluminum is high. The main function of the deoxidized modified premelted refined slag is both deoxidation and slag modification (such as increasing basicity), and requires appropriate content of lime, deoxidizers, etc.
[0025] Choose different steelmaking metallurgical processes according to different steel grades and quality requirements:
[0026] Different steelmaking metallurgical processes are selected according to the different types of steel produced, the different production paths (whether it is refined through LF furnace or RH furnace), and the different quality requirements of steel grades (differences in continuous casting castability, inclusion control requirements).
[0027] (2.1) Different steel tapping processes are used according to the different nitrogen content requirements of steel grades:
[0028] Steels with nitrogen requirements below 30ppm are tapped using a non-deoxidation process, i.e., the steel is not deoxidized, or tapped using a semi-deoxidation process, i.e., [Als] in the steel after tapping is <0.01wt%; the remaining steels are tapped using a full deoxidation process, i.e., [Als] in the steel after tapping is ≥0.01wt%.
[0029] (2.2) The composition of pre-melted refined slag is adjusted according to the different refining requirements of different steel grades:
[0030] For steel grades produced by non-deoxidation or semi-deoxidation process, deoxidation type pre-melted refined slag is used. The main components of deoxidation type pre-melted refined slag are (wt): CaO = 30-40%, CaCO 3=10-15%, metal Al = 40-50%, added to the ladle slag surface after tapping, and can also be appropriately added at the RH station according to the deoxidation effect of the top slag. According to the (FeO) content in the converter terminal slag and the amount of slag in the tapping, the amount of deoxidized pre-melted refined slag added is 1.5-2.5kg / t steel.
[0031] The steel produced by the full deoxidation process uses deoxidized modified pre-melted refined slag. The aluminum content in the refined slag is different according to the type and grade of steel, and the choice of raw materials is also very different; the main components of the deoxidized modified pre-melted refined slag are (wt): CaO = 30% ~ 40%, Al 2 O 3 =20%~30%, MgO=6%~8%, metal Al=10%~25%, burn-off=8%~10%, CaF 2 ≤4%, SiO 2 ≤6%. Add slag after steel is tapped. Adjust the amount of slag added according to the amount of slag at the converter tapping and the ∑FeO content of the slag at the end of smelting. The amount of deoxidized modified pre-melted refined slag added is 0.5-1.5kg / t steel. Deoxidize the slag; reduce the erosion of the oxidizing slag on the lining bricks of the ladle slag line; meet the performance requirements of the top slag to absorb the floating inclusions; and can replace the LF furnace refining process.
[0032] (3) Slag metallurgy process of directly adding aluminum particles to the ladle slag surface for top slag diffusion deoxidation and adjusting the aluminum content in molten steel:
[0033] Traditional post-furnace deoxidation methods for molten steel are mainly divided into precipitation deoxidation and diffusion deoxidation. The precipitation deoxidation method of adding alloys directly into molten steel has a fast deoxidation speed and high efficiency, so it is widely used. However, when alloys are directly added into molten steel, deoxidation inclusions also remain in the molten steel. On the other hand, residual elements in the alloy (such as nitrogen, oxygen, magnesium, aluminum, calcium, etc.) and inclusions carried by the alloy itself (various oxides, sulfides, etc.) also remain in the molten steel, causing secondary pollution of the molten steel. Diffusion deoxidation is rarely used because the deoxidation process relies on the diffusion of iron oxide from the molten steel to the slag phase, which is slow, time-consuming, and energy-consuming.
[0034] However, the advantage of diffusion deoxidation is that the deoxidation product is not generated in the molten steel but in the slag phase, which does not pollute the molten steel. At the same time, due to the sufficient slag deoxidation, the diffusion of oxygen in the slag into the molten steel is limited, greatly improving the cleanliness of the molten steel. Since the ladles in modern metallurgy have good bottom blowing stirring or electromagnetic stirring functions, the dynamic conditions are greatly improved, and the shortcomings of the original diffusion deoxidation process, such as slowness, time consumption and energy consumption, are eliminated. The present invention makes full use of the good stirring function of the ladles in modern metallurgy, and proposes a new slag metallurgical process of directly adding aluminum particles to the slag surface of the ladle for diffusion deoxidation and aluminum control. First, the deoxidation inclusions are left in the slag, and the purity of the molten steel is greatly improved. Second, the deoxidizer (such as aluminum particles) is thrown on the slag surface to make slag, which reduces the content of (FeO) in the slag and prevents the oxygen in the slag from diffusing into the steel, thereby ensuring a low dissolved oxygen activity in the molten steel, greatly reducing the oxide inclusions in the steel, and improving the quality of the molten steel and the product and the castability of the continuous casting molten steel.
[0035] (3.1) Slag surface deoxidation and aluminum adjustment, that is, adding aluminum particles directly to the slag surface for diffusion deoxidation and aluminum control:
[0036] After steel is tapped, the [Als] in the steel is controlled to be 0.005-0.020%. After entering the argon station, the aluminum particles are directly added to the slag surface, and cannot enter the molten steel directly. The steel / slag must be fully reacted through ladle bottom blowing and stirring, and Al is indirectly transferred into the molten steel from the slag surface; the particle size of the aluminum particles is 5-8mm. During the deoxidation and aluminum adjustment process on the slag surface, the amount of aluminum particles added is controlled to always keep [Als] in the molten steel ≥ 0.02wt%; according to the actual aluminum loss per minute in the process, the aluminum particles are added to the slag surface in two to three steps. In addition, during the deoxidation and aluminum adjustment process on the slag surface, the top slag of the ladle should remain liquid, and the C / A ratio should be 1.2-1.8, with 1.5 as the target. If the C / A ratio is low, CaO lime is added, and if it is high, Al is added. 2 O 3 Refining slag.
[0037] (3.2) Ladle bottom blowing process optimization:
[0038] The refractory material of ladle bottom blowing is Al 2 O 3 -SiO 2 -Cr 2 O 3 -ZrO 2 Argon diffusion air brick is a composite structure of mass dispersion + slit. It is mainly composed of diffusion air-permeable components, air-permeable base, and peripheral casting material. At the same time, multiple slit belts of certain width and thickness are evenly distributed around the dispersion block to increase the flow rate of the air brick by taking advantage of the large flow rate of the slit air brick. At the same time, during the refining argon blowing process, the bubbles blown out by the dispersion air brick have the characteristics of small diameter and large number compared with the slit air brick, and have excellent removal effect.
[0039] The argon blowing at the bottom of the ladle is good, and the flow rate varies with the working status and purpose of the ladle treatment; during the period of breaking the crusted top slag and molten steel refining stirring, the argon blowing stirring intensity is controlled at 100-200W / t, so that the air column formed by the bottom blowing of the ladle prompts the molten steel to move from bottom to top to form a circulation, and the mass transfer conditions are good; during the soft blowing period that promotes the growth and floating of inclusions in the molten steel, the bottom blowing argon stirring intensity is controlled at 30-50W / t, so that the upper slag-steel in the ladle maintains micro-creep (small fluctuations) to avoid exposure of the molten steel surface.
[0040] (4) After adopting the above process, the amount of aluminum used for precipitation deoxidation during steelmaking is reduced by about 10%, and the amount of aluminum used for diffusion deoxidation during refining is reduced by more than 30%; the cleanliness of the steel is greatly improved, and the TO. total oxygen content of the molten steel is reduced by at least 30%; the single-point exceeding standard rate in the steel inclusion inspection is reduced by at least 40%; in addition, the erosion of the top slag on the slag line of the ladle is reduced, the service life of the ladle is increased, and the blockage of the continuous casting nozzle is reduced.
[0041] Example 1: This low-cost refining process based on steelmaking metallurgy and slag metallurgy is described by taking the refining process of low-carbon tinplate MR steel as an example.
[0042] (1) In the process of steel tapping, aluminum-magnesium-calcium alloy is used to replace aluminum deoxidation alloy for composite deoxidation:
[0043] The aluminum-magnesium-calcium alloy used in the present invention is a molten reduction aluminum-based composite deoxidation slag-making agent, and its main components are shown in Table 1;
[0044] Table 1: Main components of aluminum-magnesium-calcium alloy
[0045] element CaO <![CDATA[Al 2 THE 3 ]]> Al <![CDATA[CaF 2 ]]> <![CDATA[CaC 2 ]]> <![CDATA[CaCO 3 ]]> MgO other content,% 20 20 45 0.5 5 0.5 8 margin
[0046] It is added into the ladle after the steel tapping starts, and other processes of the existing steel tapping process remain unchanged. Only aluminum is completely replaced by aluminum-magnesium-calcium alloy for pre-deoxidation. After steel tapping, the C / A ratio of the ladle top slag is maintained at 2.0 and MI at 0.25.
[0047] (2) After steel is tapped, pre-melted refined slag is added for re-deoxidation and white slag making:
[0048] Low carbon tinplate MR steel is a steel grade with nitrogen requirement less than 30ppm. It is produced by non-deoxidation process and uses deoxidized pre-melted refined slag. Its composition is shown in Table 2;
[0049] Table 2: Composition of deoxidized pre-melted refined slag
[0050] element CaO <![CDATA[CaCO 3 ]]> Al other content,% 40 14 45 margin
[0051] After steel is tapped, slag is added to the ladle surface. The amount added is 1.5-2.5 kg / t steel according to the (FeO) content in the converter terminal slag and the amount of slag in the steel tapping zone. In this embodiment, it is 2.4 kg / t steel.
[0052] (3) Slag surface deoxidation and aluminum adjustment process:
[0053] After steel is tapped, the [Als] in the steel is controlled to be 0.020%. After entering the argon station, aluminum particles are added directly to the slag surface, and cannot directly enter the molten steel. The particle size of the aluminum particles is 5-8mm. The amount of aluminum particles added during the slag surface deoxidation and aluminum adjustment process must always keep [Als] in the molten steel ≥ 0.02wt%; according to the actual aluminum loss per minute in the process, the aluminum particles are added to the slag surface in three steps. In addition, during the slag surface deoxidation and aluminum adjustment process, the ladle top slag should remain liquid, and the C / A ratio = 1.5 is used as the target for slag material fine-tuning.
[0054] The refractory material of ladle bottom blowing is Al 2 O 3 -SiO 2 -Cr 2 O 3 -ZrO 2 The composite structure of mass dispersion + narrow gap is used to break the top slag of the crust and during the stirring period of molten steel refining, the argon blowing stirring intensity is controlled at 100W / t; during the soft blowing period to promote the growth and floating of inclusions in the molten steel, the bottom blowing argon stirring intensity is controlled at 30W / t, and the continuous casting can be directly carried out after the composition is qualified.
[0055] After adopting the above process, molten steel can be directly cast for continuous casting, reducing the amount of aluminum used for diffusion deoxidation during refining by about 35% or more; the cleanliness of the steel is greatly improved, and the TO. total oxygen content of the molten steel is reduced by 32%; the single-point exceeding standard rate in the steel inclusion inspection is reduced by 42%, and the B coarse single-point exceeding standard rate is reduced by 36%; in addition, the erosion of the top slag on the slag line of the ladle is reduced, the service life of the ladle is increased, and the blockage of the continuous casting water nozzle is reduced.
[0056] Example 2: This low-cost refining process based on steelmaking metallurgy and slag metallurgy is described by taking the refining process of low alloy steel Q235Ti as an example.
[0057] (1) Composite deoxidation process using aluminum-magnesium-calcium alloy instead of aluminum deoxidation alloy in steel-making process The aluminum-magnesium-calcium alloy used in the present invention is a molten reduction aluminum-based composite deoxidation slag-making agent, and its main components are shown in Table 3;
[0058] Table 3: Main components of aluminum-magnesium-calcium alloy
[0059] element CaO <![CDATA[Al 2 THE 3 ]]> Al <![CDATA[CaF 2 ]]> <![CDATA[CaC 2 ]]> <![CDATA[CaCO 3 ]]> MgO other content,% 40 40 10 0.5 5.0 0.5 2.0 margin
[0060] It is added into the ladle after the steel tapping starts, and other processes of the existing steel tapping process remain unchanged. Only aluminum is completely replaced by aluminum-magnesium-calcium alloy for pre-deoxidation. After steel tapping, the C / A ratio of the ladle top slag is maintained at 1.7 and MI at 0.25.
[0061] (2) After steel is tapped, pre-melted refined slag is added for re-deoxidation and white slag making:
[0062] Low alloy steel Q235Ti belongs to the steel type produced by full deoxidation process and uses deoxidation modified pre-melted refined slag, and its composition is shown in Table 4;
[0063] Table 4: Composition of deoxidized modified pre-melted refined slag
[0064] element CaO <![CDATA[Al 2 THE 3 ]]> Al <![CDATA[SiO 2 ]]> <![CDATA[CaF 2 ]]> <![CDATA[Na 2 CO 3 ]]> MgO other content,% 30 20 25 5.0 2.5 10 6.0 margin
[0065] Add slag after steel is tapped. The amount added is adjusted according to the amount of slag at the converter tapping and the ∑FeO content of the slag at the end of smelting, generally 0.5-1.5kg / t steel. It can achieve deoxidation of the slag; reduce the erosion of the oxidizing slag on the lining bricks of the ladle slag line; meet the performance requirements of the top slag absorbing the floating inclusions; can replace the LF furnace refining process, etc., and the embodiment is 0.8kg / t steel.
[0066] (3) Slag surface deoxidation and aluminum adjustment process:
[0067] After steel is tapped, the [Als] in the steel is controlled to be 0.005%. After entering the argon station, aluminum particles are directly added to the slag surface, and cannot be directly added to the molten steel. The particle size of the aluminum particles is 5-8mm. During the deoxidation and aluminum adjustment process of the slag surface, the amount of aluminum particles added should always keep [Als] in the molten steel ≥ 0.02wt%; according to the aluminum loss per minute in the actual process, the aluminum particles are added to the slag surface in two steps. In addition, during the deoxidation and aluminum adjustment process of the slag surface, the ladle top slag should be kept in liquid state, and the slag material should be fine-tuned with the C / A ratio of 1.5 as the target.
[0068] The refractory material of ladle bottom blowing is Al 2 O 3 -SiO 2 -Cr 2 O 3 -ZrO 2 The composite structure of mass dispersion + narrow gap is used to break the top slag of the crust and during the stirring period of molten steel refining, the argon blowing stirring intensity is controlled at 200W / t; during the soft blowing period to promote the growth and floating of inclusions in the molten steel, the bottom blowing argon stirring intensity is controlled at 50W / t, and the continuous casting can be directly carried out after the composition is qualified.
[0069] After adopting the above process, molten steel can be directly cast for continuous casting, reducing the amount of aluminum used for diffusion deoxidation during refining by about 35% or more; the cleanliness of the steel is greatly improved, and the TO. total oxygen content of the molten steel is reduced by 36%; the single-point exceeding standard rate in the steel inclusion inspection is reduced by 42%, and the B coarse single-point exceeding standard rate is reduced by 40%; in addition, the erosion of the top slag on the slag line of the ladle is reduced, the service life of the ladle is increased, and the blockage of the continuous casting water nozzle is reduced.
[0070] Example 3: This low-cost refining process based on steelmaking metallurgy and slag metallurgy is described by taking the refining process of low-carbon microalloyed steel SAE1006 as an example.
[0071] (1) Composite deoxidation process using aluminum-magnesium-calcium alloy instead of aluminum deoxidation alloy during steelmaking
[0072] The aluminum-magnesium-calcium alloy used in the present invention is an electric furnace molten reduction aluminum-based composite deoxidation slag-making agent, and its main components are shown in Table 5;
[0073] Table 5: Main components of aluminum-magnesium-calcium alloy
[0074] element CaO <![CDATA[Al 2 THE 3 ]]> Al <![CDATA[CaF 2 ]]> <![CDATA[CaC 2 ]]> <![CDATA[CaCO 3 ]]> MgO other content,% 30 30 10 0.5 20 2.5 5.0 margin
[0075] It is added into the ladle after the steel tapping starts, and other processes of the existing steel tapping process remain unchanged. Only aluminum is completely replaced by aluminum-magnesium-calcium alloy for pre-deoxidation. After steel tapping, the C / A ratio of the ladle top slag is maintained at 1.8 and MI at 0.30.
[0076] (2) After steel is tapped, pre-melted refined slag is added for re-deoxidation and white slag making:
[0077] Low carbon microalloy steel SAE1006 belongs to the steel grade produced by full deoxidation process and uses deoxidized modified pre-melted refined slag. Its composition is shown in Table 6;
[0078] Table 6: Composition of deoxidized modified pre-melted refined slag
[0079] element CaO <![CDATA[Al 2 THE 3 ]]> Al <![CDATA[SiO 2 ]]> <![CDATA[CaF 2 ]]> <![CDATA[Na 2 CO 3 ]]> MgO other content,% 40 30 10 2.0 0.5 8.0 8.0 margin
[0080] Add slag after steel is tapped. The amount added is adjusted according to the amount of slag at the converter tapping and the ∑FeO content of the slag at the end of smelting, generally 0.5-1.5kg / t steel. It can achieve deoxidation of the slag; reduce the erosion of the oxidizing slag on the lining bricks of the ladle slag line; meet the performance requirements of the top slag absorbing the floating inclusions; can replace the LF furnace refining process, etc., and the embodiment is 1.4kg / t steel.
[0081] (3) Slag surface deoxidation and aluminum adjustment process:
[0082] After steel is tapped, the [Als] in the steel is controlled to be 0.005%. After entering the argon station, aluminum particles are directly added to the slag surface, and cannot be directly added to the molten steel. The particle size of the aluminum particles is 5-8mm. During the deoxidation and aluminum adjustment process of the slag surface, the amount of aluminum particles added should always keep [Als] in the molten steel ≥ 0.02wt%; according to the aluminum loss per minute in the actual process, the aluminum particles are added to the slag surface in two steps. In addition, during the deoxidation and aluminum adjustment process of the slag surface, the ladle top slag should be kept in liquid state, and the slag material should be fine-tuned with the C / A ratio of 1.5 as the target.
[0083] The refractory material of ladle bottom blowing is Al 2 O 3 -SiO2 -Cr 2 O 3 -ZrO 2 The composite structure of mass dispersion + narrow gap is used to break the top slag of the crust and the stirring period of molten steel refining, and the argon blowing stirring intensity is controlled at 150W / t; during the soft blowing period to promote the growth and floating of inclusions in the molten steel, the bottom blowing argon stirring intensity is controlled at 40W / t, and the continuous casting can be directly carried out after the composition is qualified.
[0084] After adopting the above process, molten steel can be directly cast for continuous casting, reducing the amount of aluminum used for diffusion deoxidation during refining by about 34% or more; the cleanliness of steel is greatly improved, and the TO. total oxygen content of molten steel is reduced by 38%; the single-point exceeding standard rate in steel inclusion inspection is reduced by 45%, and the D coarse single-point exceeding standard rate is reduced by 30%; in addition, the erosion of the top slag on the slag line of the ladle is reduced, the service life of the ladle is increased, the blockage of the continuous casting water nozzle is reduced, and the accidents caused by this are reduced by 80%.
Claims
1. A low-cost refining process based on steelmaking metallurgy and slag metallurgy, characterized in that: The process comprises the following steps: (1) adding aluminum-magnesium-calcium alloy as a composite deoxidizer into the ladle for composite deoxidation during steel tapping; (2) Steels with nitrogen requirements below 30 ppm are tapped using non-deoxidation or semi-deoxidation processes, while other steels are tapped using full deoxidation processes; pre-melted refined slag is added after tapping for re-deoxidation and white slag production; (3) After steel is tapped, the [Als] in the steel is controlled to be 0.005-0.020%. After entering the argon station, aluminum particles are added to the slag surface for slag surface deoxidation and aluminum adjustment. During the process, the [Als] in the molten steel is always maintained at ≥ 0.02%.
2. A low-cost refining process based on steelmaking metallurgy and slag metallurgy according to claim 1, characterized in that: In the step (1), after tapping, the ladle top slag C / A is maintained at 1.7 to 2.0 and MI is maintained at 0.25 to 0.
40.
3. A low-cost refining process based on steelmaking metallurgy and slag metallurgy according to claim 1, characterized in that: In the step (2), the viscosity of the pre-melted refined slag is 1.5-2.0 Pa·s, and the melting point is 1335-1450°C.
4. A low-cost refining process based on steelmaking metallurgy and slag metallurgy according to claim 1, characterized in that: In the step (2), the steel is produced by a non-deoxidation or semi-deoxidation process, and the pre-melted refined slag is a deoxidized pre-melted refined slag, and the addition amount is 1.5-2.5 kg / t steel; For the steel produced by the full deoxidation process, the pre-melted refined slag adopts deoxidized modified pre-melted refined slag, and the addition amount is 0.5-1.5kg / t steel.
5. A low-cost refining process based on steelmaking metallurgy and slag metallurgy according to any one of claims 1 to 4, characterized in that: In the step (3), during the slag surface deoxidation and aluminum adjustment process, the ladle top slag remains in liquid state, and the C / A ratio is 1.2 to 1.8.