Method for comprehensively utilizing high-iron and high-carbon bauxite

Through crushing, screening, dry grinding and suspension roasting, combined with gradient preheating and magnetic separation, the problem of impurities in high-speed rail high-carbon bauxite is solved, and the quality and recycling of iron concentrate and aluminum concentrate are improved. , realize efficient utilization of resources.

CN119040619APending Publication Date: 2024-11-29ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411165705.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The high content of impurities C and Fe in high-carbon bauxite of high-speed rail leads to a reduction in dissolution rate and yield of alumina, increasing the energy consumption and red mud discharge of heating equipment, and the existing methods for removing impurities and quality improvement cannot be effectively removed. Dissociation of inorganic carbon and monomers with iron-containing minerals is difficult to achieve, affecting the recovery of iron concentrate and aluminum concentrate.

Method used

By sieving and grading after crushing, dry grinding, and after merger, suspended roasting, quenching and wet grinding, combined with multi-stage gradient preheating and magnetic separation treatment, the effective decarbonization of roasted raw materials and the conversion of magnetic minerals are achieved, and iron is improved. Quality and recovery of concentrates and aluminum concentrates.

Benefits of technology

Improve the quality and recovery rate of iron concentrate and aluminum concentrate in high-speed rail high-carbon bauxite, realize the effective removal of inorganic carbon and the conversion of weak magnetic iron-containing minerals into strong magnetic minerals, reduce production costs and increase Resource utilization rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040619A_ABST
    Figure CN119040619A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of comprehensive utilization of bauxite resources, in particular to a method for comprehensively utilizing high-iron and high-carbon bauxite. The method comprises the steps that the high-iron and high-carbon bauxite is crushed and then screened and classified, and coarse-grain minerals and first fine-grain minerals are obtained; carrying out dry grinding and grading on the coarse-grained minerals to obtain second fine-grained minerals; combining the first fine-grained mineral and the second fine-grained mineral to obtain a roasting raw material; carrying out suspension roasting on the roasting raw material to obtain a roasted material; carrying out quenching, wet grinding and magnetic separation treatment on the roasted material to obtain iron ore concentrate and aluminum ore concentrate; the granularity of the first fine-grain mineral is 0.5 mm to 1.0 mm, and the granularity of the second fine-grain mineral is 0.3 mm to 0.8 mm; the suspension roasting comprises multi-stage gradient preheating and reinforced roasting, and the preheating temperature, the preheating pressure and the preheating atmosphere reducibility of the previous-stage gradient preheating are all smaller than those of the next-stage gradient preheating. The method can improve the quality and the recovery rate of the iron ore concentrate and the aluminum concentrate obtained by impurity removal and quality improvement of the high-iron and high-carbon bauxite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of comprehensive utilization of bauxite resources, and in particular to a method for comprehensive utilization of high-iron and high-carbon bauxite. Background Art

[0002] Bauxite is the main raw material for the production of alumina. At present, the bauxite to be developed and utilized in China is mainly coal-based bauxite, sedimentary bauxite, and complex bauxite resources such as high iron and high carbon. Among them, the content of impurities C and Fe in high iron and high carbon bauxite is relatively high. These C and Fe impurities will cause the Al2O3 dissolution rate and alumina production to decrease in the dissolution process of bauxite to produce alumina. At the same time, these C and Fe impurities will corrode the heating equipment used in the production, dissolution, evaporation and other processes of alumina, and will also increase the heat transfer coefficient of these heating equipment. On the one hand, the heating equipment with improved heat transfer coefficient will increase the energy consumption of the dissolution process, the steam and water consumption of the alkali elimination process, and the steam and water consumption of the evaporator. On the other hand, the heating equipment with improved heat transfer coefficient will also accelerate the scarring speed of the alumina dissolution equipment, increase the red mud discharge and reduce the resource utilization rate of bauxite. Therefore, it is necessary to remove impurities and improve the quality of high iron and high carbon bauxite before it can enter the alumina production system.

[0003] However, the current methods for removing impurities and improving the quality of high-iron and high-carbon bauxite cannot effectively remove the inorganic carbon in the high-iron and high-carbon bauxite. In addition, the mineral embedding particle size of the high-iron and high-carbon bauxite is relatively fine, and it is difficult to effectively achieve the monomer dissociation of iron-containing minerals during the impurity removal and quality improvement process. These shortcomings will lead to the inability to effectively recover the iron concentrate and aluminum concentrate in the subsequent process.

[0004] At present, the methods for removing impurities and improving the quality of high-iron and high-carbon bauxite include: (1) a method for simultaneous desulfurization and deorganicization of bauxite by reverse flotation, which method includes: first grinding and slurrying the high-sulfur and high-organic bauxite, and then adding a regulator, an activator, a desulfurization collector, a deorganic collector, and a frother to the slurryed high-sulfur and high-organic bauxite to fully mix and mineralize, so that the gangue mineral pyrite and organic matter float up through the foam carrier, while the bauxite concentrate remains in the slurry, so as to obtain a slurry containing bauxite concentrate. (2) A method for separating aluminum and iron by suspended roasting of high-iron bauxite, the method comprising: firstly crushing and grinding the high-iron bauxite and then subjecting it to a first-stage weak magnetic separation to obtain a first-stage magnetic separation tailing and a first-stage magnetic separation concentrate; subjecting the first-stage magnetic separation tailing to oxidative roasting to obtain an oxidized powder ore; then placing the oxidized powder ore in a reduction roasting furnace for reduction roasting to obtain reduced ore powder; then subjecting the reduced ore powder to a second-stage weak magnetic separation to obtain a second-stage magnetic separation concentrate and a second-stage magnetic separation tailing, respectively; then subjecting the second-stage magnetic separation tailing to a strong magnetic separation to obtain a strong magnetic separation concentrate and a strong magnetic separation tailing; then combining the strong magnetic separation concentrate and the second-stage weak magnetic separation concentrate as a finished iron concentrate, and combining the other products to obtain an aluminum concentrate. (3) A process for desulfurization and decarbonization of high-sulfur bauxite and integrated fusion processing of alumina, the process comprising: grinding the high-sulfur bauxite with a final grinding system to obtain high-sulfur bauxite powder; first introducing high-temperature hot air into a fluidized bed roasting furnace and subjecting the high-sulfur bauxite powder to fluidized bed roasting treatment to remove sulfur, carbon and part of the crystal water in the high-sulfur bauxite powder, and activating the alumina component in the high-sulfur bauxite powder to obtain a roasted, desulfurized and decarbonized aluminum concentrate. Summary of the invention

[0005] The present application provides a method for comprehensive utilization of high-iron and high-carbon bauxite to solve the following technical problem: how to improve the quality and recovery rate of iron concentrate and aluminum concentrate obtained by removing impurities and upgrading high-iron and high-carbon bauxite.

[0006] In a first aspect, the present application provides a method for comprehensive utilization of high iron and high carbon bauxite, the method comprising:

[0007] The high-iron and high-carbon bauxite is crushed, and then screened and classified to obtain coarse-grained minerals and first fine-grained minerals respectively;

[0008] dry-grinding and classifying the coarse-grained mineral to obtain a second fine-grained mineral;

[0009] combining the first fine-grained mineral and the second fine-grained mineral to obtain a roasting raw material;

[0010] The calcined raw material is subjected to suspension calcination to obtain a calcined material;

[0011] quenching the roasted material to obtain a decarburized material;

[0012] wet grinding the decarbonized material to obtain a ground material; and

[0013] The ground material is subjected to magnetic separation treatment to obtain iron concentrate and aluminum concentrate respectively;

[0014] Wherein, the particle size of the first fine-grained mineral is 0.5 mm to 1.0 mm, and the particle size of the second fine-grained mineral is 0.3 mm to 0.8 mm;

[0015] The suspended roasting includes multi-stage gradient preheating, and the multi-stage gradient preheating includes: the preheating temperature of the gradient preheating in the previous stage is less than the preheating temperature of the gradient preheating in the next stage, the preheating pressure of the gradient preheating in the previous stage is less than the preheating pressure of the gradient preheating in the next stage, and the reducing property of the preheating atmosphere of the gradient preheating in the previous stage is less than the reducing property of the preheating atmosphere of the gradient preheating in the next stage.

[0016] Optionally, the preheating temperature of the multi-stage gradient preheating is 150°C to 600°C, the preheating pressure of the multi-stage gradient preheating is -2000Pa to -400Pa, and the preheating atmosphere of the multi-stage gradient preheating includes carbon monoxide atmosphere and oxygen atmosphere, the volume of the carbon monoxide atmosphere is 1.0% to 4.0% of the total volume of the preheating atmosphere of the gradient preheating, and the volume of the oxygen atmosphere is less than or equal to 1.2% of the total volume of the preheating atmosphere of the gradient preheating.

[0017] Optionally, the gradient preheating includes primary preheating, secondary preheating, tertiary preheating, quaternary preheating and quintuple preheating;

[0018] The preheating temperature of the first stage preheating is 150°C to 200°C, the preheating temperature of the second stage preheating is 250°C to 300°C, the preheating temperature of the third stage preheating is 350°C to 400°C, the preheating temperature of the fourth stage preheating is 450°C to 500°C, and the preheating temperature of the fifth stage preheating is 550°C to 600°C;

[0019] The preheating pressure of the first-stage preheating is -2000Pa to -1700Pa, the preheating pressure of the second-stage preheating is -1700Pa to -1400Pa, the preheating pressure of the third-stage preheating is -1400Pa to -1100Pa, the preheating pressure of the fourth-stage preheating is -1100Pa to -800Pa, and the preheating pressure of the fifth-stage preheating is -800Pa to -400Pa;

[0020] The volume of the carbon monoxide atmosphere in the first-stage preheating is 1.0% to 1.6% of the total volume of the preheated atmosphere in the first-stage preheating, the volume of the carbon monoxide atmosphere in the second-stage preheating is 1.6% to 2.2% of the total volume of the preheated atmosphere in the second-stage preheating, the volume of the carbon monoxide atmosphere in the third-stage preheating is 2.2% to 2.8% of the total volume of the preheated atmosphere in the third-stage preheating, the volume of the carbon monoxide atmosphere in the fourth-stage preheating is 2.8% to 3.4% of the total volume of the preheated atmosphere in the fourth-stage preheating, and the volume of the carbon monoxide atmosphere in the fifth-stage preheating is 3.4% to 4.0% of the total volume of the preheated atmosphere in the fifth-stage preheating;

[0021] The volume of the oxygen atmosphere of the first-stage preheating is 1.0% to 1.2% of the total volume of the preheating atmosphere of the first-stage preheating, the volume of the oxygen atmosphere of the second-stage preheating is 0.8% to 1.0% of the total volume of the preheating atmosphere of the second-stage preheating, the volume of the oxygen atmosphere of the third-stage preheating is 0.1% to 0.8% of the total volume of the preheating atmosphere of the third-stage preheating, the preheating atmosphere of the fourth-stage preheating does not contain oxygen atmosphere, and the volume of the oxygen atmosphere of the fifth-stage preheating is the preheating atmosphere of the fifth-stage preheating that does not contain oxygen atmosphere.

[0022] Optionally, the first-level preheating time is 9s to 13s, the second-level preheating time is 8s to 12s, the third-level preheating time is 7s to 11s, the fourth-level preheating time is 6s to 10s, and the fifth-level preheating time is 5s to 9s.

[0023] Optionally, the suspended roasting also includes enhanced roasting, the temperature of the enhanced roasting is 600°C to 700°C, the roasting pressure of the enhanced roasting is -400Pa to -200Pa, the volume of the carbon monoxide atmosphere of the enhanced roasting is 4.0% to 4.6% of the volume of the roasting atmosphere of the enhanced roasting, the roasting atmosphere of the enhanced roasting does not contain oxygen atmosphere, and the time of the enhanced roasting is 4s to 8s.

[0024] Optionally, the weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral satisfy the relationship: m1:m2=(0.5-1):1.

[0025] Optionally, the weight of the coarse-grained minerals in the second fine-grained minerals is 90% to 98% of the total weight of the second fine-grained minerals.

[0026] Optionally, the weight of the fine-grained mineral powder in the ground material is 40% to 70% of the total weight of the ground material.

[0027] Optionally, the magnetic separation treatment includes rough magnetic separation, fine magnetic separation and sweep magnetic separation, the magnetic field strength of the rough magnetic separation is 0.2T~0.4T, the magnetic field strength of the fine magnetic separation is 0.1T~0.3T, and the magnetic field strength of the sweep magnetic separation is 0.3T~0.5T.

[0028] Optionally, the iron concentrate includes a total iron component and a first aluminum oxide component, the weight of the total iron component is greater than or equal to 62.0% of the total weight of the iron concentrate, and the weight of the first aluminum oxide component is less than or equal to 2.0% of the total weight of the iron concentrate;

[0029] The aluminum concentrate includes a carbon component and a second aluminum oxide component, the weight of the carbon component is less than or equal to 0.04% of the total weight of the aluminum concentrate, the weight of the second aluminum oxide component is greater than or equal to 65.00% of the total weight of the aluminum concentrate, and the aluminum-silicon ratio of the aluminum concentrate is greater than or equal to 6.0.

[0030] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0031] The embodiment of the present application provides a method for comprehensively utilizing high-iron and high-carbon bauxite, the method comprising: crushing the high-iron and high-carbon bauxite, and then screening and grading to obtain coarse-grained minerals and first fine-grained minerals respectively; dry-grinding and grading the coarse-grained minerals to obtain second fine-grained minerals; combining the first fine-grained minerals and the second fine-grained minerals to obtain a roasted raw material; suspending roasting the roasted raw material to obtain a roasted material; quenching the roasted material to obtain a decarbonized material; wet-grinding the decarbonized material to obtain a ground material; Magnetic separation is carried out to obtain iron concentrate and aluminum concentrate respectively; wherein the particle size of the first fine-grained mineral is 0.5mm-1.0mm, and the particle size of the second fine-grained mineral is 0.3mm-0.8mm; the suspended roasting includes multi-stage gradient preheating, and the multi-stage gradient preheating includes: the preheating temperature of the gradient preheating in the previous stage is less than the preheating temperature of the gradient preheating in the next stage, the preheating pressure of the gradient preheating in the previous stage is less than the preheating pressure of the gradient preheating in the next stage, and the reducing property of the preheating atmosphere of the gradient preheating in the previous stage is less than the reducing property of the preheating atmosphere of the gradient preheating in the next stage.In the method, the particle size of the first fine-grained mineral can be 0.5mm-1.0mm, and the particle size of the second fine-grained mineral can be 0.3mm-0.8mm, so as to promote the particle size distribution of the second fine-grained mineral to be below 0.8mm, and the combination of the first fine-grained mineral and the second fine-grained mineral can promote the particle size of the roasting raw material to be evenly distributed in the range of 0.3mm-1.0mm, and the roasting raw material distributed in the range of 0.3mm-1.0mm has good fluidity, so as to promote the roasting raw material to be fully roasted during the suspension roasting process, so that the carbon-containing minerals (such as organic carbon minerals and inorganic carbon minerals) in the roasting raw material are removed as much as possible, and the weakly magnetic iron-containing minerals can be directionally converted into strong magnetic minerals, thereby preliminarily improving the recovery effect of aluminum concentrate and iron concentrate; in addition, the suspension roasting can include multi-stage gradient preheating, and the multi-stage gradient preheating includes: the preheating temperature of the previous stage gradient preheating is less than the preheating temperature of the next stage gradient preheating, and the preheating pressure of the previous stage gradient preheating is less than the preheating pressure of the next stage gradient preheating. The preheating pressure of the first-stage gradient preheating and the reducing property of the preheating atmosphere of the previous-stage gradient preheating are lower than the reducing property of the preheating atmosphere of the subsequent-stage gradient preheating, which can cause the roasting raw materials to be always in a suspended state during the suspension roasting process. The roasting raw materials in a suspended state can, on the one hand, undergo a decomposition reaction during the suspension roasting process to effectively remove organic carbon minerals and inorganic carbon minerals in the roasting raw materials, and on the other hand, can cause the roasting raw materials to undergo a directional transformation of weakly magnetic iron-containing minerals into strongly magnetic iron-containing magnetite to reconstruct the mineral phase. Then, by quenching, a decarbonized material containing a large amount of strongly magnetic iron minerals is obtained. Then, by wet grinding, these decarbonized materials with a high content of strongly magnetic iron minerals are caused to achieve monomer dissociation, which is convenient for subsequent magnetic separation treatment. Finally, a large amount of iron concentrate with a high total iron grade and aluminum concentrate with a low impurity content (such as Fe and C) can be screened out from the ground material through magnetic separation treatment, so as to improve the quality and recovery rate of the iron concentrate and aluminum concentrate obtained by removing impurities and upgrading the high-iron and high-carbon bauxite, thereby realizing the comprehensive utilization of the high-iron and high-carbon bauxite. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0034] Figure 1 A schematic flow chart of a method for comprehensive utilization of high iron and high carbon bauxite provided in an embodiment of the present application; DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0036] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.

[0037] In this document, the terms "including" and "comprising" mean "including but not limited to". Relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0038] It should be noted that, with respect to the prior art (1) recorded in the background technology, the inventors found that: although the method can achieve the purpose of simultaneously removing sulfur minerals and organic matter from high-sulfur and high-organic bauxite, and can also remove part of the organic carbon in the high-sulfur and high-organic bauxite, it cannot play a role in removing impurities and improving the quality of inorganic carbon and iron-containing minerals in the form of carbonate in the high-sulfur and high-organic bauxite; with respect to the prior art (2) recorded in the background technology, the inventors found that: the method has the defects of high roasting temperature and complicated process flow, and because the ore grinding particle size of high-iron bauxite is fine, the material fluidity of high-iron bauxite is poor in the oxidation roasting stage, and these materials with poor fluidity are easy to be lost in various tailings components; with respect to the prior art (3) recorded in the background technology, the inventors found that: although the process can achieve the purpose of decarbonization, it still has the problems of being unable to recover the iron-containing minerals in the high-sulfur bauxite and the easy loss of the fine particle size of the high-sulfur bauxite powder.

[0039] Figure 1 A schematic flow chart of a method for comprehensive utilization of high-iron and high-carbon bauxite provided in an embodiment of the present application is exemplarily shown;

[0040] like Figure 1 As shown, the embodiment of the present application provides a method for comprehensive utilization of high iron and high carbon bauxite, the method comprising:

[0041] S1. crushing the high iron and high carbon bauxite, and then screening and grading to obtain coarse-grained minerals and first fine-grained minerals respectively;

[0042] S2. dry-grinding and classifying the coarse-grained mineral to obtain a second fine-grained mineral;

[0043] S3. combining the first fine-grained mineral and the second fine-grained mineral to obtain a roasting raw material;

[0044] S4. The calcined raw material is suspended and calcined to obtain a calcined material;

[0045] S5. The calcined material is quenched to obtain a decarburized material;

[0046] S6. The decarbonized material is wet ground to obtain a ground mineral material; and

[0047] S7. The ground material is subjected to magnetic separation to obtain iron concentrate and aluminum concentrate respectively;

[0048] Wherein, the particle size of the first fine-grained mineral is 0.5 mm to 1.0 mm, and the particle size of the second fine-grained mineral is 0.3 mm to 0.8 mm;

[0049] The suspended roasting includes multi-stage gradient preheating, and the multi-stage gradient preheating includes: the preheating temperature of the previous stage gradient preheating is less than the preheating temperature of the next stage gradient preheating, the preheating pressure of the previous stage gradient preheating is less than the preheating pressure of the next stage gradient preheating, and the reducing property of the preheating atmosphere of the previous stage gradient preheating is less than the reducing property of the preheating atmosphere of the next stage gradient preheating.

[0050] It should be noted that the particle size of the first fine-grained mineral can be 0.5mm~1.0mm, which means that the carbon-containing minerals and iron-containing minerals with smaller particle size and dissociated in the high-iron and high-carbon bauxite can be screened out through screening and grading, so as to preliminarily separate the monomer-dissociated iron-containing minerals, monomer-dissociated carbon-containing minerals and monomer-dissociated aluminum-containing minerals from the minerals that have not been dissociated, thereby reducing the amount of coarse-grained minerals entering the subsequent dry grinding and grading, and can also reduce the energy consumption of grinding while avoiding over-grinding, thereby facilitating the subsequent suspended roasting.

[0051] It should be noted that the particle size of the second fine-grained mineral can be 0.3mm to 0.8mm, which means that the iron-containing minerals, carbon-containing minerals and aluminum-containing minerals in the high-iron and high-carbon bauxite can be further screened out by dry grinding and classification to achieve monomer dissociation and separation between the three.

[0052] The particle size of the first fine-grained mineral may be 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm or 1.0 mm.

[0053] The particle size of the second fine-grained mineral may be 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm or 0.8 mm.

[0054] It should be noted that the weight of alumina in the high-iron high-carbon bauxite is more than 40% of the total weight of the high-iron high-carbon bauxite, the weight of carbon in the high-iron high-carbon bauxite is more than 1.0% of the total weight of the high-iron high-carbon bauxite, the weight of total iron components in the high-iron high-carbon bauxite is 20% to 30% of the total weight of the high-iron high-carbon bauxite, and most of the carbon in the high-iron high-carbon bauxite is inorganic carbon in the form of organic carbon and fine-grained carbonates, both of which are embedded in the high-iron high-carbon bauxite.

[0055] It should be noted that the inorganic carbon in the form of fine-grained carbonate in the high-iron and high-carbon bauxite mainly exists in the form of dolomite, calcite and siderite.

[0056] It should be noted that after dry grinding and classification, the coarser part of the mineral relative to the second fine-grained mineral can be circulated for dry grinding and classification to obtain a sufficient amount of the second fine-grained mineral.

[0057] In some optional embodiments, the preheating temperature of the multi-stage gradient preheating is 150°C to 600°C, the preheating pressure of the multi-stage gradient preheating is -2000Pa to -400Pa, and the preheating atmosphere of the multi-stage gradient preheating includes a carbon monoxide atmosphere and an oxygen atmosphere, the volume of the carbon monoxide atmosphere is 1.0% to 4.0% of the total volume of the preheating atmosphere of the gradient preheating, and the volume of the oxygen atmosphere is less than or equal to 1.2% of the total volume of the preheating atmosphere of the gradient preheating;

[0058] In these embodiments, the preheating temperature of the multi-stage gradient preheating can be 150°C to 600°C, and the preheating pressure of the multi-stage gradient preheating can be -2000Pa to -400Pa. In addition, the preheating atmosphere of the multi-stage gradient preheating can include a carbon monoxide atmosphere and an oxygen atmosphere, and the volume of the carbon monoxide atmosphere can be 1.0% to 4.0% of the total volume of the preheating atmosphere of the gradient preheating, and the volume of the oxygen atmosphere can be less than or equal to 1.2% of the total volume of the preheating atmosphere of the gradient preheating, which can promote the effective removal of carbon components from the roasting material during the suspended roasting stage, and can also promote the directional transformation of weakly magnetic iron-containing minerals in the roasting material to generate a mineral phase reconstruction of strongly magnetic iron-containing magnetite, thereby improving the magnetism and purity of the iron-containing minerals in the roasted clinker, which is beneficial to the subsequent improvement of the quality of iron concentrate and aluminum concentrate.

[0059] The preheating temperature of the gradient preheating may be 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C.

[0060] The preheating pressure of the gradient preheating may be -2000Pa, -1800Pa, -1600Pa, -1400Pa, -1200Pa, -1000Pa, -800Pa, -600Pa or -400Pa.

[0061] The volume of the carbon monoxide atmosphere may be 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5% or 4.0% of the total volume of the preheated atmosphere of the gradient preheating.

[0062] The volume of the oxygen atmosphere may be 0%, 0.5%, 1.0% or 1.2% of the total volume of the preheated atmosphere of the gradient preheating.

[0063] It should be noted that the carbon monoxide atmosphere in the preheating atmosphere of gradient preheating and the roasting atmosphere of decarbonization roasting plays an important role in the mineral phase reconstruction of iron-containing minerals in high-iron and high-iron bauxite; when the volume of the carbon monoxide atmosphere in the preheating atmosphere of gradient preheating is less than 1.0% of the total volume of the preheating atmosphere of gradient preheating, it will lead to insufficient directional conversion of weakly magnetic iron-containing minerals such as limonite and hematite in the roasting material to magnetite, thereby affecting the total iron grade and recovery rate of the iron concentrate obtained by subsequent magnetic separation treatment; when the volume of the carbon monoxide atmosphere in the preheating atmosphere of gradient preheating is greater than 4.0% of the total volume of the preheating atmosphere of gradient preheating, it will cause the volume of the preheating atmosphere of gradient preheating to have excessive carbon monoxide atmosphere, and the excessive carbon monoxide atmosphere will continue to undergo reduction reaction with the strongly magnetic iron-containing magnetite formed by the mineral phase reconstruction to generate weakly magnetic FeO (floatite) and other minerals, thereby reducing the subsequent recovery rate of the iron concentrate.

[0064] It should be noted that when the preheating temperature of the gradient preheating is less than 150°C, the directional conversion reaction of weakly magnetic iron-containing minerals in the high-iron and high-carbon bauxite cannot be carried out and the removal of carbon-containing minerals is incomplete, which will affect the conversion rate of limonite, hematite, etc. to magnetite and the removal efficiency of carbon-containing minerals; when the preheating temperature of the gradient preheating is greater than 600°C, the roasting material ore phase reconstruction will cause the generated strong magnetic magnetite to be over-reduced. For example, the strong magnetic mineral ferroferric oxide will continue to react with carbon monoxide to generate relatively weakly magnetic ferrous oxide and iron, which will affect the grade and recovery rate of the iron concentrate obtained by subsequent magnetic separation treatment, and will also cause some iron-containing minerals to be lost in the aluminum concentrate, thereby affecting the output of the iron concentrate and the quality of the aluminum concentrate. In addition, gradient preheating at too high a temperature will also increase production costs.

[0065] It should be noted that the negative pressure state of the preheating pressure is generated by using an induced draft fan to induce air. These negative pressure conditions can cause the roasting material to be in a suspended and dispersed state in the suspension roasting system; when the preheating pressure is greater than -400Pa, the roasting raw materials will be too dispersed, which will cause the loss of fine particles in the roasting material, and further affect the indicators of the suspended roasting product; when the preheating pressure is less than -2000Pa, the material will not be in a suspended and dispersed state, which will affect the decarbonization effect of the suspension roasting process and the mineral phase reconstruction effect of iron-containing minerals.

[0066] In some optional embodiments, the multi-stage gradient preheating includes primary preheating, secondary preheating, tertiary preheating, quaternary preheating and quintuple preheating;

[0067] The preheating temperature of the first stage preheating is 150°C to 200°C, the preheating temperature of the second stage preheating is 250°C to 300°C, the preheating temperature of the third stage preheating is 350°C to 400°C, the preheating temperature of the fourth stage preheating is 450°C to 500°C, and the preheating temperature of the fifth stage preheating is 550°C to 600°C;

[0068] The preheating pressure of the first-stage preheating is -2000Pa to -1700Pa, the preheating pressure of the second-stage preheating is -1700Pa to -1400Pa, the preheating pressure of the third-stage preheating is -1400Pa to -1100Pa, the preheating pressure of the fourth-stage preheating is -1100Pa to -800Pa, and the preheating pressure of the fifth-stage preheating is -800Pa to -400Pa;

[0069] The volume of the carbon monoxide atmosphere in the first-stage preheating is 1.0% to 1.6% of the total volume of the preheated atmosphere in the first-stage preheating, the volume of the carbon monoxide atmosphere in the second-stage preheating is 1.6% to 2.2% of the total volume of the preheated atmosphere in the second-stage preheating, the volume of the carbon monoxide atmosphere in the third-stage preheating is 2.2% to 2.8% of the total volume of the preheated atmosphere in the third-stage preheating, the volume of the carbon monoxide atmosphere in the fourth-stage preheating is 2.8% to 3.4% of the total volume of the preheated atmosphere in the fourth-stage preheating, and the volume of the carbon monoxide atmosphere in the fifth-stage preheating is 3.4% to 4.0% of the total volume of the preheated atmosphere in the fifth-stage preheating;

[0070] The volume of the oxygen atmosphere of the first-stage preheating is 1.0% to 1.2% of the total volume of the preheating atmosphere of the first-stage preheating, the volume of the oxygen atmosphere of the second-stage preheating is 0.8% to 1.0% of the total volume of the preheating atmosphere of the second-stage preheating, the volume of the oxygen atmosphere of the third-stage preheating is 0.1% to 0.8% of the total volume of the preheating atmosphere of the third-stage preheating, the preheating atmosphere of the fourth-stage preheating does not contain oxygen atmosphere, and the volume of the oxygen atmosphere of the fifth-stage preheating is the preheating atmosphere of the fifth-stage preheating does not contain oxygen atmosphere;

[0071] In these embodiments, the preheating temperature of the first stage preheating may be 150°C to 200°C, the preheating temperature of the second stage preheating may be 250°C to 300°C, the preheating temperature of the third stage preheating may be 350°C to 400°C, the preheating temperature of the fourth stage preheating may be 450°C to 500°C, and the preheating temperature of the fifth stage preheating may be 550°C to 600°C, and the preheating pressure of the first stage preheating may be -2000Pa to -1700Pa, the preheating pressure of the second stage preheating may be -1700Pa to -1400Pa, and the preheating pressure of the third stage preheating may be -2000Pa to -1700Pa. The preheating pressure of the first stage preheating can be -1400Pa~-1100Pa, and the preheating pressure of the fourth stage preheating is -1100Pa~-800Pa, and the preheating pressure of the fifth stage preheating can be -800Pa~-400Pa, and the volume of the carbon monoxide atmosphere of the first stage preheating can be 1.0%~1.6% of the total volume of the preheating atmosphere of the first stage preheating, and the volume of the carbon monoxide atmosphere of the second stage preheating can be 1.6%~2.2% of the total volume of the preheating atmosphere of the second stage preheating, and the volume of the carbon monoxide atmosphere of the third stage preheating can be 1.0%~1.6% of the total volume of the preheating atmosphere of the third stage preheating. The volume of the carbon monoxide atmosphere of the four-stage preheating can be 2.8% to 3.4% of the total volume of the preheated atmosphere of the four-stage preheating, and the volume of the carbon monoxide atmosphere of the five-stage preheating can be 3.4% to 4.0% of the total volume of the preheated atmosphere of the five-stage preheating, and the volume of the oxygen atmosphere of the first-stage preheating can be 1.0% to 1.2% of the total volume of the preheated atmosphere of the first-stage preheating, and the volume of the oxygen atmosphere of the second-stage preheating can be 0.8% to 1.0% of the total volume of the preheated atmosphere of the second-stage preheating, and the volume of the three-stage preheating can be 2.2% to 2.8% of the total volume of the preheated atmosphere of the four-stage preheating, and the volume of the carbon monoxide atmosphere of the five-stage preheating can be 2.8% to 3.4% of the total volume of the preheated atmosphere of the five-stage preheating, and the volume of the oxygen atmosphere of the first-stage preheating can be 1.0% to 1.2% of the total volume of the preheated atmosphere of the first-stage preheating, and the volume of the oxygen atmosphere of the second-stage preheating can be 0.8% to 1.0% of the total volume of the preheated atmosphere of the second-stage preheating, and The volume of the oxygen atmosphere in the first-stage preheating can be 0.1% to 0.8% of the total volume of the preheating atmosphere in the third-stage preheating, and the preheating atmosphere in the fourth-stage preheating does not contain oxygen atmosphere, and the volume of the oxygen atmosphere in the fifth-stage preheating can be the preheating atmosphere in the fifth-stage preheating does not contain oxygen atmosphere. The inorganic carbon components of carbon-containing minerals in the roasting raw materials can be effectively removed by the third-stage preheating, the fourth-stage preheating and the fifth-stage preheating, and the roasting raw materials are further promoted to undergo directional transformation of weakly magnetic iron-containing minerals and mineral phase reconstruction of strongly magnetic iron-containing magnetites, laying the foundation for ultimately obtaining high-quality iron concentrate and aluminum concentrate.

[0072] The preheating temperature of the primary preheating may be 150°C, 160°C, 170°C, 180°C, 190°C or 200°C.

[0073] The preheating pressure of the first-stage preheating can be -2000Pa, -1950Pa, -1900Pa, -1850Pa, -1800Pa, -1750Pa or -1700Pa.

[0074] The volume of the primary preheated carbon monoxide atmosphere may be 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5% or 1.6% of the total volume of the primary preheated atmosphere.

[0075] The volume of the primary preheated oxygen atmosphere may be 1.0%, 1.1% or 1.2% of the total volume of the primary preheated preheated atmosphere.

[0076] The preheating temperature of the secondary preheating may be 250°C, 260°C, 270°C, 280°C, 290°C or 300°C.

[0077] The preheating pressure of the secondary preheating can be -1700Pa, -1650Pa, -1600Pa, -1550Pa, -1500Pa, -1550Pa or -1400Pa.

[0078] The volume of the secondary preheated carbon monoxide atmosphere may be 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1% or 2.2% of the total volume of the secondary preheated preheated atmosphere.

[0079] The volume of the secondary preheated oxygen atmosphere may be 0.8%, 0.9% or 1.0% of the total volume of the secondary preheated preheated atmosphere.

[0080] The preheating temperature of the three-stage preheating may be 350°C, 360°C, 370°C, 380°C, 390°C or 400°C.

[0081] The preheating pressure of the three-stage preheating can be -1400Pa, -1350Pa, -1300Pa, -1250Pa, -1200Pa, -1150Pa or -1100Pa.

[0082] The volume of the three-stage preheated carbon monoxide atmosphere may be 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7% or 2.8% of the total volume of the three-stage preheated preheated atmosphere.

[0083] The volume of the tertiary preheated oxygen atmosphere may be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7% or 0.8% of the total volume of the tertiary preheated preheated atmosphere.

[0084] The preheating temperature of the four-stage preheating may be 450°C, 460°C, 470°C, 480°C, 490°C or 500°C.

[0085] The preheating pressure of the four-stage preheating can be -1100Pa, -1050Pa, -1000Pa, -950Pa, -900Pa, -850Pa or -800Pa.

[0086] The volume of the carbon monoxide atmosphere of the four-stage preheating may be 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3% or 3.4% of the total volume of the preheated atmosphere of the four-stage preheating.

[0087] The preheating temperature of the five-stage preheating may be 550°C, 560°C, 570°C, 580°C, 590°C or 600°C.

[0088] The preheating pressure of the five-stage preheating can be -800Pa, -750Pa, -700Pa, -650Pa, -600Pa, -550Pa, -500Pa, -450Pa or -400Pa.

[0089] The volume of the carbon monoxide atmosphere of the five-stage preheating may be 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9% or 4.0% of the total volume of the preheated atmosphere of the five-stage preheating.

[0090] It should be noted that if the volume of the oxygen atmosphere in the first-stage preheating is less than 1.0% of the total volume of the preheating atmosphere in the first-stage preheating, or the volume of the oxygen atmosphere in the second-stage preheating is less than 0.8% of the total volume of the preheating atmosphere in the second-stage preheating, or the volume of the oxygen atmosphere in the third-stage preheating is less than 0.1% of the total volume of the preheating atmosphere in the third-stage preheating, it will lead to incomplete reaction of organic carbon in the oxygen atmosphere to generate carbon monoxide and carbon dioxide CO or CO2 during the decarbonization process of suspension roasting, thereby affecting the quality of the aluminum concentrate; if the volume of the oxygen atmosphere in the first-stage preheating is greater than the total volume of the preheating atmosphere in the first-stage preheating, The volume of the secondary preheating oxygen atmosphere is greater than 1.2% of the total volume of the secondary preheating atmosphere or the volume of the tertiary preheating oxygen atmosphere is greater than 1.0% of the total volume of the tertiary preheating atmosphere, or the volume of the tertiary preheating oxygen atmosphere is greater than 0.8% of the total volume of the tertiary preheating atmosphere, which will result in the organic carbon in the roasting raw material being unable to completely consume the oxygen in the oxygen atmosphere, and the excess oxygen in the oxygen atmosphere will directly oxidize the strongly magnetic iron minerals such as magnetite already generated in the roasting material into weakly magnetic iron minerals, thereby affecting the mineral phase reconstruction process of the iron-containing minerals in the roasting material during suspension roasting, and further affecting the grade and recovery rate of the iron concentrate obtained by subsequent magnetic separation treatment.

[0091] In some optional embodiments, the time for the first-level preheating is 9s to 3s, the time for the second-level preheating is 8s to 12s, the time for the third-level preheating is 7s to 11s, the time for the fourth-level preheating is 6s to 10s, and the time for the fifth-level preheating is 5s to 9s.

[0092] In these embodiments, the time for the first-stage preheating can be 9s to 13s, the time for the second-stage preheating can be 8s to 12s, and the time for the third-stage preheating can be 7s to 11s. The organic carbon component of the carbon-containing minerals in the roasting material can be effectively removed by the first-stage preheating, the second-stage preheating and the third-stage preheating, and the roasting raw materials are prompted to initially undergo a directional transformation of weakly magnetic iron-containing minerals into strongly magnetic iron-containing magnetites to reconstruct the mineral phase, so as to ultimately obtain iron ore and aluminum concentrate with high purity and content; in addition, the time for the fourth-stage preheating can be 6s to 10s and the time for the fifth-stage preheating can be 5s to 9s. The inorganic carbon component of the carbon-containing minerals in the roasting material can be effectively removed by the fourth-stage preheating and the fifth-stage preheating, and the roasting raw materials are prompted to further undergo a directional transformation of weakly magnetic iron-containing minerals into strongly magnetic iron-containing magnetites to reconstruct the mineral phase, so as to ultimately obtain iron ore and aluminum concentrate with high purity and content.

[0093] The time for the first stage preheating can be 9s, 10s, 11s, 12s or 13s.

[0094] The secondary preheating time can be 8s, 9s, 10s, 11s or 12s.

[0095] The time of the three-stage preheating can be 7s, 8s, 9s, 10s or 11s.

[0096] The time of the four-stage preheating can be 6s, 7s, 8s, 9s or 10s.

[0097] The five-stage preheating time may be 5s, 6s, 7s, 8s or 9s.

[0098] In some optional embodiments, the suspended roasting also includes enhanced roasting, the temperature of the enhanced roasting is 600°C to 700°C, the roasting pressure of the enhanced roasting is -400Pa to -200Pa, the volume of the carbon monoxide atmosphere of the enhanced roasting is 4.0% to 4.6% of the volume of the roasting atmosphere of the enhanced roasting, the roasting atmosphere of the enhanced roasting does not contain oxygen atmosphere, and the time of the enhanced roasting is 4s to 8s.

[0099] In these embodiments, suspended roasting may also include enhanced roasting, the temperature of the enhanced roasting may be 600°C to 700°C, and the roasting pressure of the enhanced roasting may be -400Pa to -200Pa, and the volume of the carbon monoxide atmosphere of the enhanced roasting may be 4.0% to 4.6% of the volume of the roasting atmosphere of the enhanced roasting, and the roasting atmosphere of the enhanced roasting may not contain an oxygen atmosphere, which can further remove the inorganic carbon components of the carbon-containing minerals in the roasting material, and promote the roasting material to completely undergo the directional transformation of weakly magnetic iron-containing minerals and the mineral phase reconstruction of strongly magnetic iron-containing magnetite, so as to ultimately obtain high-quality iron concentrate and aluminum concentrate.

[0100] The temperature of the decarburization roasting can be 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C or 700°C.

[0101] The decarburization roasting pressure may be -400Pa, -350Pa, -300Pa, -250Pa or -200Pa.

[0102] The volume of the carbon monoxide atmosphere of the decarburization roasting can be 4.0%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5% or 4.6% of the total volume of the roasting atmosphere of the decarburization roasting.

[0103] It should be noted that the suspended roasting as a whole can include three stages: decarbonization roasting for organic carbon-containing minerals, decarbonization roasting for inorganic carbon-containing minerals, and magnetization roasting for iron-containing minerals. Among them, the decarbonization roasting for organic carbon-containing minerals can be completed in the first stage preheating, the second stage preheating, and the third stage preheating, while the decarbonization roasting for inorganic carbon-containing minerals and the magnetization roasting for iron-containing minerals can be completed in the fourth stage preheating, the fifth stage preheating, and the intensive roasting.

[0104] In some optional embodiments, the weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral satisfy the relationship: m1:m2=(0.5-1):1;

[0105] In these embodiments, the weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral can satisfy the relationship: m1:m2=(0.5~1):1, which can facilitate the first fine-grained mineral and the second fine-grained mineral to be combined to obtain a roasted material with a particle size between 0.3mm and 1.0mm, and the roasted material in the range of 0.3mm to 1.0mm has good fluidity, so as to facilitate the roasted material to be fully roasted during the suspended roasting process, so as to facilitate the dissociation and separation of carbon-containing minerals and iron-containing minerals in the roasted material from other minerals as much as possible, thereby preliminarily improving the recovery effect of aluminum concentrate and iron concentrate.

[0106] The weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral may satisfy the relationship: m1:m2=0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1 or 1:1.

[0107] In some optional embodiments, the weight of the coarse-grained minerals in the second fine-grained minerals is greater than or equal to 90% to 98% of the total weight of the second fine-grained minerals;

[0108] In these embodiments, the weight of the coarse-grained minerals in the second fine-grained mineral can be greater than or equal to 90% to 98% of the total weight of the second fine-grained mineral, which can promote the sufficient monomer dissociation and separation between the iron-containing minerals, carbon-containing minerals and aluminum-containing minerals in the high-iron and high-carbon bauxite in the dry grinding and classification process, thereby improving the subsequent recovery rates of aluminum concentrate and iron concentrate.

[0109] The weight of the coarse-grained mineral in the second fine-grained mineral may be 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97% or 98% of the total weight of the second fine-grained mineral.

[0110] It should be noted that the particle size of the coarse-grained mineral is ≥ 0.5 mm

[0111] It should be noted that, when the weight of coarse-grained minerals in the second fine-grained minerals is greater than 98% of the total weight of the second fine-grained minerals, the dissociation of iron-containing minerals, carbon-containing minerals and aluminum-containing minerals in the high-iron and high-carbon bauxite will be poor, which may lead to poor decarburization and iron removal effects in suspended roasting; when the weight of coarse-grained minerals in the second fine-grained minerals is less than 90% of the total weight of the second fine-grained minerals, the high-iron and high-carbon bauxite will be over-grinded. The over-grinded high-iron and high-carbon bauxite contains a large amount of fine-grained mineral powder, which will affect the fluidity of the material. The high-iron and high-carbon bauxite with poor fluidity will affect the decarburization and iron removal effects in the suspended roasting stage.

[0112] In some optional embodiments, the weight of the fine-grained mineral powder in the ground mineral material is 40% to 70% of the total weight of the ground mineral material;

[0113] In these embodiments, the weight of the fine-grained mineral powder in the ground material can be 40% to 70% of the total weight of the ground material, which can promote the monomer dissociation of iron-containing minerals, aluminum-containing minerals and other gangue minerals in the decarbonized material as much as possible, so as to improve the separation effect of subsequent magnetic separation treatment.

[0114] The weight of the fine-grained mineral powder in the ground material may be 40%, 45%, 50%, 55%, 60%, 65% or 70% of the total weight of the ground material.

[0115] It should be noted that, when the weight of the fine-grained mineral powder in the grinding material is less than 40% of the total weight of the grinding material, it means that the monomer dissociation of the iron-containing minerals, aluminum-containing minerals and other gangue minerals in the grinding material is not good, which affects the quality of the final iron concentrate and aluminum concentrate; when the weight of the fine-grained mineral powder in the grinding material is greater than 70% of the total weight of the grinding material, it will cause over-grinding of the iron-containing minerals and aluminum-containing minerals in the grinding material, and the over-grinded iron-containing minerals will be lost in the aluminum concentrate, which will not only reduce the yield of the final iron concentrate, but also affect the quality of the final aluminum concentrate, and at the same time increase the energy consumption of dry grinding and classification.

[0116] It should be noted that the particle size of the fine-grained mineral powder is ≤0.044 mm.

[0117] In some optional embodiments, the magnetic separation treatment includes rough magnetic separation, fine magnetic separation and scavenging magnetic separation, the magnetic field strength of the rough magnetic separation is 0.2T to 0.4T, the magnetic field strength of the fine magnetic separation is 0.1T to 0.3T, and the magnetic field strength of the scavenging magnetic separation is 0.3T to 0.5T;

[0118] In these embodiments, the magnetic separation treatment may include rough magnetic separation, fine magnetic separation and scavenging magnetic separation, and the magnetic field intensity of the rough magnetic separation may be 0.2T to 0.4T, and the magnetic field intensity of the fine magnetic separation may be 0.1T to 0.3T, and the magnetic field intensity of the scavenging magnetic separation may be 0.3T to 0.5T. The magnetic separation treatment may be used to increase the total iron content of the final magnetically separated iron concentrate and to increase the total iron recovery rate of the final iron concentrate. In addition, the magnetic separation treatment may be used to reduce the content of iron impurities in the aluminum concentrate, thereby obtaining a high-quality aluminum concentrate with excellent magnetic separation iron removal indicators.

[0119] The magnetic field strength of the rough magnetic separation can be 0.2T, 0.3T or 0.4T.

[0120] The magnetic field strength of the magnetic separation can be 0.1T, 0.2T or 0.3T.

[0121] The magnetic field strength of the magnetic separation can be 0.3T, 0.4T or 0.5T.

[0122] It should be noted that when the magnetic field intensity of the rough magnetic separation is less than 0.2T, although the total iron grade of the iron concentrate after the rough magnetic separation will be improved, the recovery rate of the iron concentrate after the rough magnetic separation will be low and the iron impurities in the aluminum concentrate will be high; when the magnetic field intensity of the rough magnetic separation is greater than 0.4T, it will lead to serious mechanical inclusions in the rough magnetic separation process, thereby greatly reducing the total iron content of the iron concentrate after the rough magnetic separation, affecting the magnetic separation effect of the rough magnetic separation.

[0123] It should be noted that when the magnetic field intensity of magnetic separation is less than 0.1T, the magnetic field intensity of magnetic separation will be weak, resulting in a decrease in the yield of iron concentrate and high iron impurities in aluminum concentrate; when the magnetic field intensity of magnetic separation is greater than 0.3T, the total iron content of the iron concentrate will be reduced, which can affect the quality of the iron concentrate.

[0124] It should be noted that when the magnetic field intensity of the magnetic separation is less than 0.3T, the magnetic field intensity of the magnetic separation will be too small. The magnetic separation with too small magnetic field intensity cannot recover the iron-containing minerals in the ground material, which will affect the recovery rate of the iron concentrate and increase the iron impurities in the aluminum concentrate; when the magnetic field intensity of the magnetic separation is greater than 0.5T, the ground material and aluminum-containing mineral veins will be mechanically included in the iron concentrate product, thereby reducing the total iron content of the iron concentrate, thereby reducing the quality of the iron concentrate and the yield of the aluminum concentrate.

[0125] In some optional embodiments, the iron concentrate includes a total iron component and a first aluminum oxide component, the weight of the total iron component is greater than or equal to 62.0% of the total weight of the iron concentrate, and the weight of the first aluminum oxide component is less than or equal to 2.0% of the total weight of the iron concentrate;

[0126] The aluminum concentrate comprises a carbon component and a second aluminum oxide component, the weight of the carbon component is less than or equal to 0.04% of the total weight of the aluminum concentrate, the weight of the second aluminum oxide component is greater than or equal to 65.00% of the total weight of the aluminum concentrate, and the aluminum-silicon ratio of the aluminum concentrate is greater than or equal to 6.0;

[0127] In these embodiments, the iron concentrate may include a total iron component and a first alumina component, and the weight of the total iron component may be greater than or equal to 62.0% of the total weight of the iron concentrate, and the weight of the first alumina component may be less than or equal to 2.0% of the total weight of the iron concentrate, which can enable the iron concentrate to have sufficient iron elements and a small amount of harmful impurities of alumina to meet the requirements of the iron concentrate as a steel smelting, thereby indicating that the iron concentrate has a good grade; in addition, the aluminum concentrate may include a carbon component and a second alumina component, and the weight of the carbon component may be less than or equal to 0.04% of the total weight of the aluminum concentrate, and the weight of the second alumina component may be greater than or equal to 65.00% of the total weight of the aluminum concentrate, and the aluminum-silicon ratio of the aluminum concentrate is greater than or equal to 6.0, which can enable the aluminum concentrate to have sufficient aluminum elements and a small amount of carbon impurities and a good aluminum-silicon ratio, thereby indicating that the obtained aluminum concentrate has good quality to meet the demand for aluminum concentrate as a raw material for alumina production, thereby realizing the comprehensive utilization of high-iron and high-carbon bauxite.

[0128] It should be noted that the first alumina component and the second alumina component merely represent the alumina components in different substances, and data such as the purity and particle size of the alumina may be the same or different.

[0129] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.

[0130] Example 1

[0131] A high-iron high-carbon bauxite in a certain place in Henan Province was selected. The chemical composition of the high-iron high-carbon bauxite includes, by mass fraction, Al2O3: 42.33%, SiO2: 8.51%, TFe: 21.36%, C: 2.74%. The mineral composition of the high-iron high-carbon bauxite includes diaspore and a small amount of gibbsite. The vein minerals in the mineral composition of the high-iron high-carbon bauxite include chlorite, dolomite, calcite and kaolinite. The iron in the high-iron high-carbon bauxite is mainly present in the form of limonite, hematite and a small amount of siderite, and the carbon in the high-iron high-carbon bauxite is mainly present in the form of organic carbon and inorganic carbon (the inorganic carbon is mainly present in mineral components such as dolomite, calcite and siderite), wherein the weight of organic carbon is 48.81% of the weight of carbon in the high-iron high-carbon bauxite.

[0132] like Figure 1 As shown, a method for comprehensively utilizing high-iron and high-carbon bauxite comprises:

[0133] S1. crushing the high iron and high carbon bauxite, and then screening and grading to obtain coarse-grained minerals and first fine-grained minerals respectively;

[0134] S2. dry-grinding and classifying the coarse-grained mineral to obtain a second fine-grained mineral;

[0135] S3. combining the first fine-grained mineral and the second fine-grained mineral to obtain a roasting raw material;

[0136] S4. The calcined raw material is suspended and calcined to obtain a calcined material;

[0137] S5. The calcined material is quenched to obtain a decarburized material;

[0138] S6. The decarbonized material is wet ground to obtain a ground mineral material;

[0139] S7. The ground material is subjected to magnetic separation to obtain iron concentrate and aluminum concentrate respectively;

[0140] Among them, the target particle size of screening classification is 0.5m~0.8mm (at this time 0.5mm≤the particle size of the first fine mineral≤0.8mm), and the target particle size of dry grinding classification is 0.3mm~0.8mm (at this time 0.3mm≤the particle size of the second fine mineral≤0.8mm).

[0141] The number of gradient preheating stages is 5, the preheating temperature of the first stage preheating is 170°C, the preheating pressure of the first stage preheating is -1850Pa, the volume of the carbon monoxide atmosphere of the first stage preheating is 1.0% of the total volume of the preheating atmosphere of the first stage preheating, and the volume of the oxygen atmosphere of the first stage preheating is 1.1% of the total volume of the preheating atmosphere of the first stage preheating;

[0142] The preheating temperature of the secondary preheating is 295°C, the preheating pressure of the secondary preheating is -1600Pa, the volume of the carbon monoxide atmosphere of the secondary preheating is 1.6% of the total volume of the preheating atmosphere of the secondary preheating, and the volume of the oxygen atmosphere of the secondary preheating is 0.9% of the total volume of the preheating atmosphere of the secondary preheating;

[0143] The preheating temperature of the three-stage preheating is 382°C, the preheating pressure of the three-stage preheating is -1210Pa, the volume of the carbon monoxide atmosphere of the three-stage preheating is 2.2% of the total volume of the preheating atmosphere of the three-stage preheating, and the volume of the oxygen atmosphere of the three-stage preheating is 0.2% of the total volume of the preheating atmosphere of the three-stage preheating;

[0144] The preheating temperature of the four-stage preheating is 480°C, the preheating pressure of the four-stage preheating is -960Pa, the volume of the carbon monoxide atmosphere of the four-stage preheating is 2.9% of the total volume of the preheating atmosphere of the four-stage preheating, and the preheating atmosphere of the four-stage preheating does not contain an oxygen atmosphere;

[0145] The preheating temperature of the five-stage preheating is 583°C, the preheating pressure of the five-stage preheating is -501Pa, the volume of the carbon monoxide atmosphere of the five-stage preheating is 3.6% of the volume of the preheating atmosphere of the five-stage preheating, and the preheating atmosphere of the five-stage preheating does not contain oxygen atmosphere.

[0146] The first-level preheating time is 10s, the second-level preheating time is 8s, the third-level preheating time is 7s, the fourth-level preheating time is 7s, and the fifth-level preheating time is 6s.

[0147] The temperature of the enhanced calcination is 683°C, the calcination pressure is -240Pa, the volume of the carbon monoxide atmosphere of the enhanced calcination is 4.20% of the total volume of the calcination atmosphere of the enhanced calcination, the volume of the oxygen atmosphere of the enhanced calcination is 0% of the total volume of the calcination atmosphere of the enhanced calcination, and the decarburization calcination time is 5s.

[0148] The weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral satisfy the relationship: m1:m2=1:1.

[0149] The weight of the coarse-grained minerals in the second fine-grained minerals is 95.75% of the total weight of the second fine-grained minerals; and the particle size of the coarse-grained minerals is ≥0.5 mm.

[0150] The weight of the fine-grained mineral powder in the ground material is 51.76% of the total weight of the ground material; the particle size of the fine-grained mineral powder is ≤0.044 mm.

[0151] The magnetic separation treatment includes rough magnetic separation, fine magnetic separation and scavenging magnetic separation. The magnetic field intensity of rough magnetic separation is 0.25T, the magnetic field intensity of fine magnetic separation is 0.2T, and the magnetic field intensity of scavenging magnetic separation is 0.35T.

[0152] The specific indicators of the aluminum concentrate and iron concentrate obtained by this method are shown in Table 1.

[0153] Table 1 Component contents of the product of Example 1

[0154]

[0155] It can be seen from Table 1 that after the high-iron and high-carbon bauxite in a certain place in Henan is treated by the method provided in the embodiment of the present application, an aluminum concentrate with a yield of 61.22%, an Al2O3 content of 68.38%, an A / S of 6.44, a TFe content of 4.87% and an impurity C content of 0.03% can be obtained, as well as an iron concentrate for steel smelting with a yield of 29.63%, a TFe content of 62.03% and an impurity Al2O3 content of 1.58%. This shows that the aluminum concentrate obtained by this method not only removes harmful impurities, but also increases the alumina content and A / S, and at the same time obtains high-quality iron concentrate, thereby realizing the comprehensive utilization of high-iron and high-carbon bauxite.

[0156] Example 2

[0157] Based on the contents disclosed in Example 1, the following modifications are further made:

[0158] A high-iron high-carbon bauxite in a certain place in Shanxi Province was selected. The chemical composition of the high-iron high-carbon bauxite includes, by mass fraction, Al2O3: 41.08%, SiO2: 9.06%, TFe: 24.16%, C: 1.86%. The mineral composition of the high-iron high-carbon bauxite includes diaspore and a small amount of gibbsite. The vein minerals in the mineral composition of the high-iron high-carbon bauxite include chlorite, kaolinite, illite, dolomite, calcite, anatase and rutile. The iron in the high-iron high-carbon bauxite is mainly present in the form of limonite and hematite in the original ore, and the carbon in the high-iron high-carbon bauxite is mainly present in the form of organic carbon and inorganic carbon (the inorganic carbon is mainly present in mineral components such as dolomite and calcite), wherein the weight of organic carbon is 51.33% of the total weight of carbon in the high-iron high-carbon bauxite.

[0159] The target particle size of screening classification is 0.6mm~0.7mm (at this time 0.6mm≤the particle size of the first fine mineral≤0.7mm), and the target particle size of dry grinding classification is 0.4mm~0.6mm (at this time 0.4mm≤the particle size of the second fine mineral≤0.6mm).

[0160] The preheating temperature of the first-stage preheating is 165° C., the preheating pressure of the first-stage preheating is −1780 Pa, the volume of the carbon monoxide atmosphere of the first-stage preheating is 1.10% of the total volume of the preheating atmosphere of the first-stage preheating, and the volume of the oxygen atmosphere of the first-stage preheating is 1.07% of the total volume of the preheating atmosphere of the first-stage preheating;

[0161] The preheating temperature of the secondary preheating is 282°C, the preheating pressure of the secondary preheating is -1630Pa, the volume of the carbon monoxide atmosphere of the secondary preheating is 1.70% of the total volume of the preheating atmosphere of the secondary preheating, and the volume of the oxygen atmosphere of the secondary preheating is 0.8% of the total volume of the preheating atmosphere of the secondary preheating;

[0162] The preheating temperature of the three-stage preheating is 376°C, the preheating pressure of the three-stage preheating is -1170Pa, the volume of the carbon monoxide atmosphere of the three-stage preheating is 2.4% of the total volume of the preheating atmosphere of the three-stage preheating, and the volume of the oxygen atmosphere of the three-stage preheating is 0.20% of the total volume of the preheating atmosphere of the three-stage preheating;

[0163] The preheating temperature of the four-stage preheating is 495°C, the preheating pressure of the four-stage preheating is -890Pa, the volume of the carbon monoxide atmosphere of the four-stage preheating is 3.2% of the total volume of the preheating atmosphere of the four-stage preheating, and the preheating atmosphere of the four-stage preheating does not contain an oxygen atmosphere;

[0164] The preheating temperature of the five-stage preheating is 600°C, the preheating pressure of the five-stage preheating is -720Pa, the volume of the carbon monoxide atmosphere of the five-stage preheating is 3.8% of the volume of the preheating atmosphere of the five-stage preheating, and the preheating atmosphere of the five-stage preheating does not contain oxygen atmosphere.

[0165] The first-level preheating time is 12s, the second-level preheating time is 11s, the third-level preheating time is 9s, the fourth-level preheating time is 7s, and the fifth-level preheating time is 6s.

[0166] The temperature of the enhanced calcination is 695°C, the calcination pressure of the enhanced calcination is -310Pa, the volume of the carbon monoxide atmosphere of the enhanced calcination is 4.15% of the volume of the calcination atmosphere of the enhanced calcination, the calcination atmosphere of the enhanced calcination does not contain oxygen atmosphere, and the enhanced calcination time is 4s.

[0167] The weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral satisfy the relationship: m1:m2=0.7:1.

[0168] The weight of the coarse-grained minerals in the second fine-grained minerals is 95.75% of the total weight of the second fine-grained minerals; and the particle size of the coarse-grained minerals is ≥0.5 mm.

[0169] The weight of the fine-grained mineral powder in the ground material is 61.22% of the total weight of the ground material; the particle size of the fine-grained mineral powder is ≤0.044 mm.

[0170] The magnetic separation treatment includes rough magnetic separation, fine magnetic separation and scavenging magnetic separation. The magnetic field intensity of rough magnetic separation is 0.30T, the magnetic field intensity of fine magnetic separation is 0.25T, and the magnetic field intensity of scavenging magnetic separation is 0.40T.

[0171] The specific indicators of the aluminum concentrate and iron concentrate obtained by this method are shown in Table 2.

[0172] Table 2 Component contents of the product of Example 2

[0173]

[0174]

[0175] It can be seen from Table 2 that after the high-iron and high-carbon bauxite in a certain place in Shanxi is treated by the method provided in the embodiment of the present application, an aluminum concentrate with a yield of 58.19%, an Al2O3 content of 69.58%, an A / S of 6.10, a TFe content of 6.10% and an impurity C content of 0.02% can be obtained, as well as an iron concentrate for steel smelting with a yield of 33.14%, a TFe content of 62.80% and an impurity Al2O3 content of 1.78%. It shows that the aluminum concentrate obtained by this method not only removes harmful impurities, but also increases the alumina content and A / S, and at the same time obtains high-quality iron concentrate, thereby realizing the comprehensive utilization of high-iron and high-carbon bauxite.

[0176] Example 3

[0177] Based on the contents disclosed in Example 1, the following modifications are further made:

[0178] A high-iron and high-carbon bauxite from a place in Guangxi was selected. Calculated by mass fraction, the chemical composition of the high-iron and high-carbon bauxite includes: Al2O3: 47.33%, SiO2: 10.77%, TFe: 20.66%, C: 3.12%. The available minerals in the mineral composition of the high-iron and high-carbon bauxite include diaspore, a small amount of gibbsite and boehmite. The vein minerals in the mineral composition of the high-iron and high-carbon bauxite include kaolinite, pyrophyllite, calcite, illite, dolomite, calcite, anatase and rutile. The iron in the high-iron and high-carbon bauxite is mainly present in the original ore in the form of limonite and hematite, while the carbon in the high-iron and high-carbon bauxite is mainly present in the form of organic carbon and inorganic carbon (the inorganic carbon is mainly present in mineral components such as dolomite and calcite), of which the weight of organic carbon is 60.33% of the weight of carbon in the high-iron and high-carbon bauxite.

[0179] The target particle size of screening classification is 0.5mm~0.9mm (at this time 0.5mm≤the particle size of the first fine mineral≤0.9mm), and the target particle size of dry grinding classification is 0.4mm~0.8mm (at this time 0.4mm≤the particle size of the second fine mineral≤0.8mm).

[0180] The preheating temperature of the first stage preheating is 175°C, the preheating pressure of the first stage preheating is -1880Pa, the volume of the carbon monoxide atmosphere of the first stage preheating is 1.30% of the total volume of the preheating atmosphere of the first stage preheating, and the volume of the oxygen atmosphere of the first stage preheating is 1.05% of the total volume of the preheating atmosphere of the first stage preheating;

[0181] The preheating temperature of the secondary preheating is 293°C, the preheating pressure of the secondary preheating is -1555Pa, the volume of the carbon monoxide atmosphere of the secondary preheating is 2.10% of the total volume of the preheating atmosphere of the secondary preheating, and the volume of the oxygen atmosphere of the secondary preheating is 0.75% of the total volume of the preheating atmosphere of the secondary preheating;

[0182] The preheating temperature of the three-stage preheating is 390°C, the preheating pressure of the three-stage preheating is -1345Pa, the volume of the carbon monoxide atmosphere of the three-stage preheating is 2.60% of the total volume of the preheating atmosphere of the three-stage preheating, and the volume of the oxygen atmosphere of the three-stage preheating is 0.35% of the total volume of the preheating atmosphere of the three-stage preheating;

[0183] The preheating temperature of the four-stage preheating is 486°C, the preheating pressure of the four-stage preheating is -1025Pa, the volume of the carbon monoxide atmosphere of the four-stage preheating is 2.95% of the total volume of the preheating atmosphere of the four-stage preheating, and the preheating atmosphere of the four-stage preheating does not contain an oxygen atmosphere;

[0184] The preheating temperature of the five-stage preheating is 595°C, the preheating pressure of the five-stage preheating is -779Pa, the volume of the carbon monoxide atmosphere of the five-stage preheating is 3.62% of the volume of the preheating atmosphere of the five-stage preheating, and the preheating atmosphere of the five-stage preheating does not contain oxygen atmosphere.

[0185] The first-level preheating time is 9s, the second-level preheating time is 8s, the third-level preheating time is 8s, the fourth-level preheating time is 7s, and the fifth-level preheating time is 5s.

[0186] The temperature of the enhanced calcination is 674°C, the calcination pressure of the enhanced calcination is -389Pa, the volume of the carbon monoxide atmosphere of the enhanced calcination is 4.41% of the total volume of the calcination atmosphere of the enhanced calcination, the calcination atmosphere of the enhanced calcination does not contain oxygen atmosphere, and the enhanced calcination time is 4s.

[0187] The weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral satisfy the relationship: m1:m2=0.7:1.

[0188] The weight of the coarse-grained minerals in the second fine-grained minerals is 92.33% of the total weight of the second fine-grained minerals; and the particle size of the coarse-grained minerals is ≥0.5 mm.

[0189] The weight of the fine-grained mineral powder in the ground material is 49.82% of the total weight of the ground material; the particle size of the fine-grained mineral powder is ≤0.044 mm.

[0190] The magnetic separation treatment includes rough magnetic separation, fine magnetic separation and scavenging magnetic separation. The magnetic field intensity of rough magnetic separation is 0.25T, the magnetic field intensity of fine magnetic separation is 0.20T, and the magnetic field intensity of scavenging magnetic separation is 0.30T.

[0191] The specific indicators of the aluminum concentrate and iron concentrate obtained by this method are shown in Table 3.

[0192] Table 3 Component contents of the product of Example 3

[0193]

[0194] It can be seen from Table 3 that after the high-iron and high-carbon bauxite in a certain place in Guangxi is treated by the method provided in the embodiment of the present application, an aluminum concentrate with a yield of 61.28%, an Al2O3 content of 76.79%, an A / S of 6.02, a TFe content of 3.90% and an impurity C content of 0.04% can be obtained, as well as an iron concentrate for steel smelting with a yield of 29.47%, a TFe content of 62.01% and an impurity Al2O3 content of 0.93%. This shows that the aluminum concentrate obtained by this method not only removes harmful impurities, but also increases the alumina content and A / S, and at the same time obtains high-quality iron concentrate, thereby realizing the comprehensive utilization of high-iron and high-carbon bauxite.

[0195] Example 4

[0196] A high iron and high carbon bauxite in the BOFFA mining area of ​​Guinea was selected. The chemical composition of the high iron and high carbon bauxite includes, by mass fraction: Al2O3: 46.78%, SiO2: 2.87%, TFe: 24.68%, C: 4.16%. The available minerals in the mineral composition of the high iron and high carbon bauxite include gibbsite, and the gangue minerals are mainly kaolinite, rutile, dolomite, etc. The iron in the high iron and high carbon bauxite is mainly present in the original ore in the form of limonite and hematite, and the carbon in the high iron and high carbon bauxite is mainly present in the form of organic carbon, and there is a small amount of inorganic carbon (the inorganic carbon is mainly present in dolomite), wherein the weight of the organic carbon is 82.87% of the weight of the carbon in the high iron and high carbon bauxite.

[0197] The target particle size of screening classification is 0.6mm~1.0mm (at this time 0.6mm≤the particle size of the first fine mineral≤1.0mm), and the target particle size of dry grinding classification is 0.3mm~0.7mm (0.3mm≤the particle size of the second fine mineral≤0.7mm).

[0198] The preheating temperature of the first-stage preheating is 197° C., the preheating pressure of the first-stage preheating is −1975 Pa, the volume of the carbon monoxide atmosphere of the first-stage preheating is 1.10% of the total volume of the preheating atmosphere of the first-stage preheating, and the volume of the oxygen atmosphere of the first-stage preheating is 1.20% of the total volume of the preheating atmosphere of the first-stage preheating;

[0199] The preheating temperature of the secondary preheating is 289° C., the preheating pressure of the secondary preheating is −1693 Pa, the volume of the carbon monoxide atmosphere of the secondary preheating is 1.79% of the total volume of the preheating atmosphere of the secondary preheating, and the volume of the oxygen atmosphere of the secondary preheating is 0.81% of the total volume of the preheating atmosphere of the secondary preheating;

[0200] The preheating temperature of the three-stage preheating is 387°C, the preheating pressure of the three-stage preheating is -1384Pa, the volume of the carbon monoxide atmosphere of the three-stage preheating is 2.65% of the total volume of the preheating atmosphere of the three-stage preheating, and the volume of the oxygen atmosphere of the three-stage preheating is 0.38% of the total volume of the preheating atmosphere of the three-stage preheating;

[0201] The preheating temperature of the four-stage preheating is 491°C, the preheating pressure of the four-stage preheating is -1074Pa, the volume of the carbon monoxide atmosphere of the four-stage preheating is 3.2% of the total volume of the preheating atmosphere of the four-stage preheating, and the preheating atmosphere of the four-stage preheating does not contain an oxygen atmosphere;

[0202] The preheating temperature of the five-stage preheating is 587°C, the preheating pressure of the five-stage preheating is -784Pa, the volume of the carbon monoxide atmosphere of the five-stage preheating is 3.85% of the total volume of the preheating atmosphere of the five-stage preheating, and the preheating atmosphere of the five-stage preheating does not contain oxygen atmosphere.

[0203] The first-level preheating time is 10s, the second-level preheating time is 9s, the third-level preheating time is 8s, the fourth-level preheating time is 6s, and the fifth-level preheating time is 5s.

[0204] The temperature of the enhanced calcination is 695°C, the calcination pressure of the enhanced calcination is -400Pa, the volume of the carbon monoxide atmosphere of the enhanced calcination is 4.39% of the total volume of the calcination atmosphere of the enhanced calcination, the calcination atmosphere of the enhanced calcination does not contain oxygen atmosphere, and the enhanced calcination time is 5s.

[0205] The weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral satisfy the relationship: m1:m2=1:1.

[0206] The weight of the coarse-grained minerals in the second fine-grained minerals is 91.75% of the total weight of the second fine-grained minerals; and the particle size of the coarse-grained minerals is ≥0.5 mm.

[0207] The weight of the fine-grained mineral powder in the ground material is 59.73% of the total weight of the ground material; the particle size of the fine-grained mineral powder is ≤0.044 mm.

[0208] The magnetic separation treatment includes rough magnetic separation, fine magnetic separation and scavenging magnetic separation. The magnetic field intensity of rough magnetic separation is 0.35T, the magnetic field intensity of fine magnetic separation is 0.25T, and the magnetic field intensity of scavenging magnetic separation is 0.5T.

[0209] The specific indicators of the aluminum concentrate and iron concentrate obtained by this method are shown in Table 4.

[0210] Table 4 Component contents of the product of Example 4

[0211]

[0212] It can be seen from Table 4 that after a certain high-iron and high-carbon bauxite in the BOFFA mining area of ​​Guinea is treated by the method provided in the embodiment of the present application, an aluminum concentrate with a yield of 58.09%, an Al2O3 content of 79.63%, an A / S of 20.31, a TFe content of 9%, and an impurity C content of 0.02% can be obtained, as well as an iron concentrate for steel smelting with a yield of 29.06%, a TFe content of 66.91%, and an impurity Al2O3 content of 1.80%. It shows that the aluminum concentrate obtained by this method not only removes harmful impurities, but also increases the alumina content and A / S, and at the same time obtains high-quality iron concentrate, thereby realizing the comprehensive utilization of high-iron and high-carbon bauxite.

[0213] Example 5

[0214] A high iron and high carbon bauxite in the Koumia mining area of ​​Guinea was selected. The chemical composition of the high iron and high carbon bauxite includes, by mass fraction: Al2O3: 51.78%, SiO2: 5.01%, TFe: 18.54%, C: 3.41%. The available minerals in the mineral composition of the high iron and high carbon bauxite include gibbsite, and the gangue minerals are mainly kaolinite, rutile, dolomite, etc. The iron in the high iron and high carbon bauxite is mainly present in the original ore in the form of limonite and hematite, and the carbon in the high iron and high carbon bauxite is mainly present in the form of organic carbon, and there is a small amount of inorganic carbon (the inorganic carbon is mainly present in dolomite), wherein the weight of the organic carbon is 84.71% of the weight of the carbon in the high iron and high carbon bauxite.

[0215] The target particle size of screening classification is 0.5mm~0.7mm (at this time 0.5mm≤the particle size of the first fine mineral≤0.7mm), and the target particle size of dry grinding classification is 0.3mm~0.6mm (at this time 0.6mm≤the particle size of the second fine mineral≤0.6mm).

[0216] The preheating temperature of the first-stage preheating is 165° C., the preheating pressure of the first-stage preheating is −1651 Pa, the volume of the carbon monoxide atmosphere of the first-stage preheating is 1.21% of the volume of the preheating atmosphere of the first-stage preheating, and the volume of the oxygen atmosphere of the first-stage preheating is 1.15% of the total volume of the preheating atmosphere of the first-stage preheating;

[0217] The preheating temperature of the secondary preheating is 267°C, the preheating pressure of the secondary preheating is -1513Pa, the volume of the carbon monoxide atmosphere of the secondary preheating is 1.82% of the total volume of the preheating atmosphere of the secondary preheating, and the volume of the oxygen atmosphere of the secondary preheating is 0.86% of the total volume of the preheating atmosphere of the secondary preheating;

[0218] The preheating temperature of the three-stage preheating is 362°C, the preheating pressure of the three-stage preheating is -1257Pa, the volume of the carbon monoxide atmosphere of the three-stage preheating is 2.45% of the total volume of the preheating atmosphere of the three-stage preheating, and the volume of the oxygen atmosphere of the three-stage preheating is 0.23% of the total volume of the preheating atmosphere of the three-stage preheating;

[0219] The preheating temperature of the four-stage preheating is 471°C, the preheating pressure of the four-stage preheating is -985Pa, the volume of the carbon monoxide atmosphere of the four-stage preheating is 2.96% of the total volume of the preheating atmosphere of the four-stage preheating, and the preheating atmosphere of the four-stage preheating does not contain an oxygen atmosphere;

[0220] The preheating temperature of the five-stage preheating is 591°C, the preheating pressure of the five-stage preheating is -694Pa, ​​the volume of the carbon monoxide atmosphere of the five-stage preheating is 4.0% of the total volume of the preheating atmosphere of the five-stage preheating, and the preheating atmosphere of the five-stage preheating does not contain oxygen atmosphere.

[0221] The first-level preheating time is 13s, the second-level preheating time is 11s, the third-level preheating time is 9s, the fourth-level preheating time is 8s, and the fifth-level preheating time is 6s.

[0222] The temperature of the enhanced calcination is 673°C, the calcination pressure of the enhanced calcination is -320Pa, the volume of the carbon monoxide atmosphere of the enhanced calcination is 4.0% of the total volume of the calcination atmosphere of the enhanced calcination, the calcination atmosphere of the enhanced calcination does not contain oxygen atmosphere, and the enhanced calcination time is 6s.

[0223] The weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral satisfy the relationship: m1:m2=0.7:1.

[0224] The weight of the coarse-grained minerals in the second fine-grained minerals is 97.58% of the total weight of the second fine-grained minerals; and the particle size of the coarse-grained minerals is ≥0.3 mm.

[0225] The weight of the fine-grained mineral powder in the ground material is 66.71% of the total weight of the ground material; the particle size of the fine-grained mineral powder is ≤0.044 mm.

[0226] The magnetic separation treatment includes rough magnetic separation, fine magnetic separation and scavenging magnetic separation. The magnetic field intensity of rough magnetic separation is 0.39T, the magnetic field intensity of fine magnetic separation is 0.28T, and the magnetic field intensity of scavenging magnetic separation is 0.45T.

[0227] The specific indicators of the aluminum concentrate and iron concentrate obtained by this method are shown in Table 5.

[0228] Table 5 Component contents of the product of Example 5

[0229]

[0230] It can be seen from Table 5 that after a certain high-iron and high-carbon bauxite from an Australian mine is treated by the method provided in the embodiment of the present application, an aluminum concentrate with a yield of 65.33%, an Al2O3 content of 78.63%, an A / S of 13.04, a TFe content of 8.02% and an impurity C content of 0.01% can be obtained, as well as an iron concentrate for steel smelting with a yield of 20.92%, a TFe content of 63.55%, and an impurity Al2O3 content of 1.96%. This shows that the aluminum concentrate obtained by this method not only removes harmful impurities, but also increases the alumina content and A / S, and at the same time obtains high-quality iron concentrate, thereby realizing the comprehensive utilization of high-iron and high-carbon bauxite.

[0231] Comparative Example 1

[0232] Based on the contents disclosed in Example 1, further modifications are made:

[0233] The components of the product obtained by using the method described in the prior art (2) in the background art are shown in Table 6.

[0234] Table 6 Component contents of the product of Comparative Example 1

[0235]

[0236] Comparative Example 2

[0237] Based on the contents disclosed in Example 2, further modifications are made:

[0238] The components of the product obtained by processing using the method described in the prior art (2) in the background art are shown in Table 7.

[0239] Table 7 Component contents of the product of Comparative Example 2

[0240]

[0241] Comparative Example 3

[0242] Based on the contents disclosed in Example 3, further modifications are made:

[0243] The components of the product obtained by processing using the method described in the prior art (2) in the background art are shown in Table 8.

[0244] Table 8 Component contents of the product of Comparative Example 3

[0245]

[0246] Comparative Example 4

[0247] Based on the contents disclosed in Example 4, further modifications are made:

[0248] The components of the product obtained by using the method described in the prior art (2) in the background art are shown in Table 9.

[0249] Table 9 Component contents of the product of Comparative Example 4

[0250]

[0251] Comparative Example 5

[0252] Based on the contents disclosed in Example 5, further modifications are made:

[0253] The components of the product obtained by processing using the method described in the prior art (2) in the background art are shown in Table 10.

[0254] Table 10 Component contents of the product of Comparative Example 5

[0255]

[0256]

[0257] Comparative Example 6

[0258] Based on the contents disclosed in Example 1, the following modifications are further made:

[0259] The target particle size of the screening classification is 0.2-0.5 mm (at this time 0.2 mm ≤ the particle size of the first fine mineral ≤ 0.5 mm), and the target particle size of the dry grinding classification is 0.1 mm-0.3 mm (at this time 0.1 mm ≤ the particle size of the second fine mineral ≤ 0.3 mm). The component contents of the obtained products are shown in Table 11.

[0260] Table 11 Component contents of the product of Comparative Example 6

[0261]

[0262] Comparative Example 7

[0263] Based on the contents disclosed in Example 1, the following modifications are further made:

[0264] The target particle size of the screening classification is 1.5 mm to 2.5 mm (at this time 1.5 mm ≤ the particle size of the first fine mineral ≤ 2.5 mm), and the target particle size of the dry grinding classification is 1.0 mm to 1.5 mm (at this time 1.0 mm ≤ the particle size of the second fine mineral ≤ 1.5 mm). The component contents of the obtained products are shown in Table 12.

[0265] Table 12 Component contents of the product of Comparative Example 7

[0266]

[0267] Comparative Example 8

[0268] Based on the contents disclosed in Example 1, the following modifications are further made:

[0269] The preheating temperature of the first-stage preheating is 100°C, the preheating pressure of the first-stage preheating is -2500Pa, the volume of the carbon monoxide atmosphere of the first-stage preheating is 0.5% of the total volume of the preheating atmosphere of the first-stage preheating, and the volume of the oxygen atmosphere of the first-stage preheating is 0.5% of the total volume of the preheating atmosphere of the first-stage preheating.

[0270] The preheating temperature of the secondary preheating is 200°C, the preheating pressure of the secondary preheating is -2000Pa, the volume of the carbon monoxide atmosphere of the secondary preheating is 1.2% of the total volume of the preheating atmosphere of the secondary preheating, and the volume of the oxygen atmosphere of the secondary preheating is 0.5% of the total volume of the preheating atmosphere of the secondary preheating.

[0271] The preheating temperature of the three-stage preheating is 300°C, the preheating pressure of the three-stage preheating is -1500Pa, the volume of the carbon monoxide atmosphere of the three-stage preheating is 2.0% of the total volume of the preheating atmosphere of the three-stage preheating, and the volume of the oxygen atmosphere of the three-stage preheating is 0% of the total volume of the preheating atmosphere of the three-stage preheating. The component contents of the obtained products are shown in Table 13.

[0272] Table 13 Component contents of the product of Comparative Example 8

[0273]

[0274] Comparative Example 9

[0275] Based on the contents disclosed in Example 1, the following modifications are further made:

[0276] The preheating temperature of the first-stage preheating is 250°C, the preheating pressure of the first-stage preheating is -1500Pa, the volume of the carbon monoxide atmosphere of the first-stage preheating is 2.0% of the total volume of the preheating atmosphere of the first-stage preheating, and the volume of the oxygen atmosphere of the first-stage preheating is 2.0% of the total volume of the preheating atmosphere of the first-stage preheating.

[0277] The preheating temperature of the secondary preheating is 350°C, the preheating pressure of the secondary preheating is -1000Pa, the volume of the carbon monoxide atmosphere of the secondary preheating is 3.0% of the total volume of the preheating atmosphere of the secondary preheating, and the volume of the oxygen atmosphere of the secondary preheating is 2.0% of the total volume of the preheating atmosphere of the secondary preheating.

[0278] The preheating temperature of the three-stage preheating is 450°C, the preheating pressure of the three-stage preheating is -1000 Pa, the volume of the carbon monoxide atmosphere of the three-stage preheating is 3.0% of the total volume of the preheating atmosphere of the three-stage preheating, and the volume of the oxygen atmosphere of the three-stage preheating is 1.0% of the total volume of the preheating atmosphere of the two-stage preheating. The component contents of the obtained products are shown in Table 14.

[0279] Table 14 Component contents of the product of Comparative Example 9

[0280]

[0281] Comparative Example 10

[0282] Based on the contents disclosed in Example 1, the following modifications are further made:

[0283] The preheating temperature of the four-stage preheating is 400° C., the preheating pressure of the four-stage preheating is −1500 Pa, and the volume of the carbon monoxide atmosphere of the four-stage preheating is 2.2% of the total volume of the preheating atmosphere of the four-stage preheating.

[0284] The preheating temperature of the five-stage preheating is 500° C., the preheating pressure of the five-stage preheating is −900 Pa, and the volume of the carbon monoxide atmosphere of the five-stage preheating is 3.0% of the total volume of the preheating atmosphere of the five-stage preheating. The component contents of the obtained products are shown in Table 15.

[0285] Table 15 Component contents of the product of Comparative Example 10

[0286]

[0287]

[0288] Comparative Example 11

[0289] Based on the contents disclosed in Example 1, the following modifications are further made:

[0290] The preheating temperature of the four-stage preheating is 600° C., the preheating pressure of the four-stage preheating is −500 Pa, and the volume of the carbon monoxide atmosphere of the four-stage preheating is 4.0% of the total volume of the preheating atmosphere of the four-stage preheating.

[0291] The preheating temperature of the five-stage preheating is 650°C, the preheating pressure of the five-stage preheating is -300 Pa, and the volume of the carbon monoxide atmosphere of the five-stage preheating is 5.0% of the total volume of the preheating atmosphere of the five-stage preheating. The component contents of the obtained products are shown in Table 16.

[0292] Table 16 Component contents of the product of Comparative Example 11

[0293]

[0294] Comparative Example 12

[0295] Based on the contents disclosed in Example 1, the following modifications are further made:

[0296] The temperature of the enhanced calcination was 500°C, the calcination pressure of the enhanced calcination was -600 Pa, and the volume of the carbon monoxide atmosphere of the enhanced calcination was 2.0% of the volume of the calcination atmosphere of the enhanced calcination. The component contents of the obtained products are shown in Table 17.

[0297] Table 17 Component contents of the product of Comparative Example 12

[0298]

[0299] Comparative Example 13

[0300] Based on the contents disclosed in Example 1, the following modifications are further made:

[0301] The temperature of the enhanced calcination is 800°C, the calcination pressure of the enhanced calcination is -100 Pa, and the volume of the carbon monoxide atmosphere of the enhanced calcination is 5.0% of the volume of the calcination atmosphere of the enhanced calcination. The component contents of the obtained products are shown in Table 18.

[0302] Table 18 Component contents of the product of Comparative Example 13

[0303]

[0304] Related test and effect data:

[0305] The product indicators obtained by the methods provided in the embodiments and comparative examples are statistically analyzed, and the results are shown in Table 19 below.

[0306] Table 19 Comparison of product indicators obtained by the embodiment and the comparative example

[0307]

[0308]

[0309]

[0310] As can be seen from the above table, the embodiment of the present application provides a method for comprehensive utilization of high-iron and high-carbon bauxite. The iron concentrate obtained by the method has a TFe content of ≥62.01% and a low impurity Al2O3 content, which can meet the requirements of GB / T36704-2018 on the national quality standard for iron concentrate. In addition, the recovery rate of iron concentrate recovered from high-iron and high-carbon bauxite by the method is high; in addition, the Al2O3 content in the aluminum concentrate obtained by the method is greater than 65%, and the content of impurity carbon or impurity iron is significantly reduced, and the A / S of the ore is also significantly improved, which shows that the method realizes the comprehensive utilization of high-iron and high-carbon bauxite; while Comparative Examples 1 to Comparative Examples 5 use traditional methods and target the same high-iron and high-carbon bauxite. The obtained iron concentrate has a heavy TFe content of 53.94% to 56.50%, which is much lower than the TFe content in the iron concentrate obtained in the embodiment, and the impurity Al2O3 content in the iron concentrate obtained in Comparative Examples 1 to 5 is also much higher than that in the iron concentrate obtained in the embodiment; in addition, the yield and recovery rate of the aluminum concentrate obtained in Comparative Examples 1 to 5 are also much lower than those in the embodiment, which may be because the fine grinding and dry magnetic separation adopted in Comparative Examples 1 to 5 will cause mechanical inclusions, and at the same time, the grinding fineness of Comparative Examples 1 to 5 is too fine, resulting in the loss of fine-grained minerals in the bag dust collection device during the suspended magnetic roasting process. Therefore, Comparative Examples 1 to 5 will also have the problem of loss of fine-grained ore particles.

[0311] By comparing the test data of Comparative Examples 6 and 7 with Example 1, it can be seen that the total iron grade of the iron concentrate obtained in Comparative Example 6 when the particle size of the first fine-grained mineral and the particle size of the second fine-grained mineral are finer is slightly lower than that in Example 1, and the iron impurity content of the aluminum concentrate is higher than that in Example 1. At the same time, Comparative Example 6 also suffers from the loss of fine-grained material (the loss output is 3.72%), while in Comparative Example 7 when the particle size of the first fine-grained mineral and the particle size of the second fine-grained mineral are coarser, the particle size of the roasting raw material will be coarser, and the coarser roasting raw material will have a monomer dissociation difference with each mineral, and the existence of the monomer dissociation difference will reduce the decarburization effect and iron removal effect of the suspended roasting process. From the data, the total iron content of the iron concentrate obtained in Comparative Example 7 is 2.97% lower than that in Example 1, and the impurity content (impurity carbon and impurity iron) of the aluminum concentrate is higher than that in Comparative Example 1. It can be clearly seen that the particle size of the first fine-grained mineral and the particle size of the second fine-grained mineral are too coarse, which will lead to poor decarburization and iron removal effects of suspended roasting. It can be seen from this that the particle size of the first fine-grained mineral and the particle size range of the second fine-grained mineral provided in the embodiment of the present application are optimal.

[0312] By analyzing the data of Comparative Examples 8, 9 and Example 1, it is found that the indicators of iron concentrate and aluminum concentrate in Comparative Examples 8 and 9 are lower than those in Example 1. This is because the conditions of primary preheating, secondary preheating and tertiary preheating are too low, which will affect the removal rate of carbon-containing minerals (especially organic carbon) in the roasting raw materials, thereby increasing the impurity carbon content in the aluminum concentrate, while the conditions of primary preheating, secondary preheating and tertiary preheating are too high, which will cause the generated strong magnetic iron minerals to react with excessive oxygen to produce weak magnetic iron minerals, which will increase the iron impurity content of the aluminum concentrate while reducing the output and total iron content of the iron concentrate, thereby affecting the quality of the iron concentrate and the aluminum concentrate. Therefore, the conditions of primary preheating, secondary preheating and tertiary preheating provided in this application are the optimal parameters.

[0313] By analyzing the data of Comparative Example 10, Comparative Example 11 and Example 1, it is found that the indicators of iron concentrate and aluminum concentrate in Comparative Example 10 and Comparative Example 11 are not as good as those in Example 1. This is because the conditions of the four-stage preheating and the five-stage preheating are too low, which will affect the removal rate of carbon-containing minerals (especially inorganic carbon) in the roasting raw materials, thereby increasing the impurity carbon content in the aluminum concentrate; while the conditions of the four-stage preheating and the five-stage preheating are too high, which will cause the generated strong magnetic iron minerals to undergo over-reduction reaction with excessive carbon monoxide to produce weak magnetic iron minerals, which will increase the iron impurity content of the aluminum concentrate while reducing the output and total iron content of the iron concentrate, thereby affecting the quality of the iron concentrate and the aluminum concentrate. Therefore, the conditions of the four-stage preheating and the five-stage preheating provided in this application are the optimal parameters.

[0314] By analyzing the data of Comparative Example 12, Comparative Example 13 and Example 1, it is found that the indicators of iron concentrate and aluminum concentrate in Comparative Example 12 and Comparative Example 13 are much lower than those in Example 1. This is because reducing the conditions for enhanced roasting will affect the removal rate of carbon-containing minerals (especially inorganic carbon) in the roasting raw materials and reduce the reaction process of directional conversion of weakly magnetic iron-containing minerals into strongly magnetic minerals, which will not only lead to an increase in the content of impurities (such as iron and carbon) in the aluminum concentrate, but also reduce the total iron grade and output of the iron concentrate; and if the conditions for enhanced roasting are too high, the generated strongly magnetic iron minerals and excessive carbon monoxide will undergo a violent over-reduction reaction under higher temperature conditions, and produce a large amount of weakly magnetic iron minerals, which will reduce the output and total iron content of the iron concentrate while increasing the iron impurity content of the aluminum concentrate, thereby affecting the quality of the iron concentrate and the aluminum concentrate. Therefore, the conditions for enhanced roasting provided in this application are the optimal parameters.

[0315] In summary, the embodiments of the present application provide a method for comprehensive utilization of high-iron and high-carbon bauxite, which can increase the recovery rate of iron concentrate in the high-iron and high-carbon bauxite to more than 20% and the recovery rate of aluminum concentrate in the high-iron and high-carbon bauxite to more than 50%.

[0316] In addition, an embodiment of the present application provides a method for comprehensive utilization of high-iron and high-carbon bauxite. The method uses a method of crushing first and then screening and grading, and dry grinding and grading in series, which can promote the particle size of the roasting raw material to be distributed within the range of 0.1mm to 0.9mm as much as possible. The roasting raw material distributed in the range of 0.1mm to 0.8mm has good fluidity, so as to promote the roasting raw material to be fully roasted during the suspended roasting process, thereby promoting the inorganic carbon minerals and iron-containing minerals in the roasting raw material to be separated from other minerals as much as possible, thereby preliminarily improving the recovery effect of aluminum concentrate and iron concentrate. In addition, the method of crushing first and then screening and grading, and dry grinding and grading in series can also save the industrial cost of grinding ore.

[0317] In addition, an embodiment of the present application provides a method for comprehensive utilization of high-iron and high-carbon bauxite. By setting preheating temperatures, preheating pressures and preheating gas atmospheres with different gradient preheating in a suspended roasting system, the roasting raw materials can be kept in a suspended state. The roasting raw materials in a suspended state can undergo decomposition reactions of organic carbon and inorganic carbon during the suspended roasting process to effectively remove organic carbon minerals and inorganic carbon minerals in the roasting raw materials. On the other hand, the roasting raw materials can undergo directional transformation of weakly magnetic iron-containing minerals into strongly magnetic iron-containing magnetites to reconstruct the mineral phase. The use of suspended roasting can remove impurity carbon-containing minerals in iron-containing minerals without producing polluting products. At the same time, the aluminum concentrate and iron concentrate obtained by the method do not contain chemical agents, and therefore do not affect the subsequent use of aluminum concentrate as a raw material for alumina production and the use of iron concentrate as a raw material for steel production, thereby realizing the comprehensive utilization of high-iron and high-carbon bauxite.

[0318] In addition, a method for comprehensive utilization of high-iron and high-carbon bauxite provided in an embodiment of the present application can obtain iron concentrate and aluminum concentrate with a good recovery rate, which can not only increase the utilization rate of high-iron and high-carbon bauxite, but also provide high-quality raw materials for the steel industry, thereby realizing the comprehensive utilization of high-iron and high-carbon bauxite. In addition, this method has the advantages of low cost, high economic benefit, good quality of iron concentrate, high resource utilization, mature and stable process, and environmental friendliness.

[0319] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.

Claims

1. A method for comprehensive utilization of high iron and high carbon bauxite, characterized in that: The method comprises: The high-iron and high-carbon bauxite is crushed, and then screened and classified to obtain coarse-grained minerals and first fine-grained minerals respectively; dry-grinding and classifying the coarse-grained mineral to obtain a second fine-grained mineral; combining the first fine-grained mineral and the second fine-grained mineral to obtain a roasting raw material; The calcined raw material is subjected to suspension calcination to obtain a calcined material; quenching the roasted material to obtain a decarburized material; wet grinding the decarbonized material to obtain a ground material; and The ground material is subjected to magnetic separation treatment to obtain iron concentrate and aluminum concentrate respectively; Wherein, the particle size of the first fine-grained mineral is 0.5 mm to 1.0 mm, and the particle size of the second fine-grained mineral is 0.3 mm to 0.8 mm; The suspended roasting includes multi-stage gradient preheating, and the multi-stage gradient preheating includes: the preheating temperature of the previous stage gradient preheating is less than the preheating temperature of the next stage gradient preheating, the preheating pressure of the previous stage gradient preheating is less than the preheating pressure of the next stage gradient preheating, and the reducing property of the preheating atmosphere of the previous stage gradient preheating is less than the reducing property of the preheating atmosphere of the next stage gradient preheating.

2. The method according to claim 1, characterized in that The preheating temperature of the multi-stage gradient preheating is 150°C to 600°C from low to high, the preheating pressure of the multi-stage gradient preheating is -2000Pa to -400Pa from low to high, and the preheating atmosphere of the multi-stage gradient preheating includes carbon monoxide atmosphere and oxygen atmosphere. The volume of the carbon monoxide atmosphere is 1.0% to 4.0% of the total volume of the preheating atmosphere, and the volume of the oxygen atmosphere is less than or equal to 1.2% of the total volume of the preheating atmosphere.

3. The method according to claim 2, characterized in that The multi-stage gradient preheating includes primary preheating, secondary preheating, tertiary preheating, quaternary preheating and quintuple preheating; The preheating temperature of the first stage preheating is 150°C to 200°C, the preheating temperature of the second stage preheating is 250°C to 300°C, the preheating temperature of the third stage preheating is 350°C to 400°C, the preheating temperature of the fourth stage preheating is 450°C to 500°C, and the preheating temperature of the fifth stage preheating is 550°C to 600°C; The preheating pressure of the first-stage preheating is -2000Pa to -1700Pa, the preheating pressure of the second-stage preheating is -1700Pa to -1400Pa, the preheating pressure of the third-stage preheating is -1400Pa to -1100Pa, the preheating pressure of the fourth-stage preheating is -1100Pa to -800Pa, and the preheating pressure of the fifth-stage preheating is -800Pa to -400Pa; The volume of the carbon monoxide atmosphere in the first-stage preheating is 1.0% to 1.6% of the total volume of the preheated atmosphere in the first-stage preheating, the volume of the carbon monoxide atmosphere in the second-stage preheating is 1.6% to 2.2% of the total volume of the preheated atmosphere in the second-stage preheating, the volume of the carbon monoxide atmosphere in the third-stage preheating is 2.2% to 2.8% of the total volume of the preheated atmosphere in the third-stage preheating, the volume of the carbon monoxide atmosphere in the fourth-stage preheating is 2.8% to 3.4% of the total volume of the preheated atmosphere in the fourth-stage preheating, and the volume of the carbon monoxide atmosphere in the fifth-stage preheating is 3.4% to 4.0% of the total volume of the preheated atmosphere in the fifth-stage preheating; The volume of the oxygen atmosphere of the first-stage preheating is 1.0% to 1.2% of the total volume of the preheating atmosphere of the first-stage preheating, the volume of the oxygen atmosphere of the second-stage preheating is 0.8% to 1.0% of the total volume of the preheating atmosphere of the second-stage preheating, the volume of the oxygen atmosphere of the third-stage preheating is 0.1% to 0.8% of the total volume of the preheating atmosphere of the third-stage preheating, the preheating atmosphere of the fourth-stage preheating does not contain oxygen atmosphere, and the volume of the oxygen atmosphere of the fifth-stage preheating is the preheating atmosphere of the fifth-stage preheating that does not contain oxygen atmosphere.

4. The method according to claim 3, characterized in that The time for the first-stage preheating is 9s to 13s, the time for the second-stage preheating is 8s to 12s, the time for the third-stage preheating is 7s to 11s, the time for the fourth-stage preheating is 6s to 10s, and the time for the fifth-stage preheating is 5s to 9s.

5. The method according to claim 1, characterized in that The suspended roasting also includes enhanced roasting, the temperature of the enhanced roasting is 600°C to 700°C, the roasting pressure of the enhanced roasting is -400Pa to -200Pa, the volume of the carbon monoxide atmosphere of the enhanced roasting is 4.0% to 4.6% of the volume of the roasting atmosphere of the enhanced roasting, the roasting atmosphere of the enhanced furnace roasting does not contain oxygen atmosphere, and the time of the enhanced roasting is 4s to 8s.

6. The method according to claim 1, characterized in that The weight m1 of the first fine-grained mineral and the weight m2 of the second fine-grained mineral satisfy the relationship: m1:m2=(0.5-1):

1.

7. The method according to claim 1, characterized in that The weight of the coarse-grained minerals in the second fine-grained minerals is 90% to 98% of the total weight of the second fine-grained minerals.

8. The method according to claim 1, characterized in that The weight of the fine-grained mineral powder in the ground mineral material is 40% to 70% of the total weight of the ground mineral material.

9. The method according to claim 1, characterized in that: The magnetic separation treatment includes rough magnetic separation, fine magnetic separation and scavenging magnetic separation. The magnetic field strength of the rough magnetic separation is 0.2T to 0.4T, the magnetic field strength of the fine magnetic separation is 0.1T to 0.3T, and the magnetic field strength of the scavenging magnetic separation is 0.3T to 0.5T.

10. The method according to claim 1, characterized in that The iron concentrate comprises a total iron component and a first aluminum oxide component, the weight of the total iron component is greater than or equal to 62.0% of the total weight of the iron concentrate, and the weight of the first aluminum oxide component is less than or equal to 2.0% of the total weight of the iron concentrate; The aluminum concentrate includes a carbon component and a second aluminum oxide component, the weight of the carbon component is less than or equal to 0.04% of the total weight of the aluminum concentrate, the weight of the second aluminum oxide component is greater than or equal to 65.00% of the total weight of the aluminum concentrate, and the aluminum-silicon ratio of the aluminum concentrate is greater than or equal to 6.0.

Citation Information

Cited By

  • Method for separating and recovering aluminum and iron from high-carbon high-iron diaspore type bauxite

    CN122706937A

  • Method for separating and recovering aluminum and iron from high-carbon high-iron diaspore type bauxite