Selective leaching method of lithium iron phosphate battery black powder and method for recycling battery grade lithium carbonate

Through high-temperature leaching of nitric acid and multi-step purification treatment, the leaching selectivity and purity of lithium in lithium iron phosphate batteries are improved, and the problem of large lithium loss in the prior art is solved, and efficient lithium carbonate recovery is achieved.

CN119040637APending Publication Date: 2024-11-29CENT SOUTH UNIV

Patent Information

Application Number
CN202411253560.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the existing lithium iron phosphate battery recycling technology, the leaching selectivity of lithium is not high, resulting in large losses of lithium, and the impurity removal process will cause large losses of lithium, which will not reach the purity of the battery level.

Method used

Using the high-temperature leaching method of nitric acid, combining phosphorus and iron compounds as adjusters, controlling the leaching conditions, improving the leaching selectivity of lithium, and reducing the loss of lithium through multiple steps of purification and impurity removal processes, and finally obtaining battery-grade lithium carbonate .

Benefits of technology

The leaching rate of lithium is achieved at more than 99.5%, the selectivity is reached more than 75%, the lithium loss is less than 0.3% during the impurity removal process, and the purity of lithium carbonate reaches the battery level standard.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040637A_ABST
    Figure CN119040637A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of waste battery recovery, and discloses a selective leaching method of lithium iron phosphate battery black powder and a method for recovering battery-grade lithium carbonate from the lithium iron phosphate battery black powder. A nitric acid solution is added into the lithium iron phosphate battery black powder, leaching is carried out at 105-200 DEG C, and selective leaching of lithium is achieved. In the nitric acid leaching process, a phosphorus compound or an iron compound is added as a regulator, so that the selective leaching effect of lithium can be further improved. In the process of recovering lithium carbonate, firstly, a calcium-containing reagent is actively introduced to reduce lithium loss, and then, the battery-grade lithium carbonate is obtained by sectional impurity removal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste battery recycling, and specifically relates to a method for leaching black powder from waste lithium iron phosphate batteries and a method for directly recovering battery-grade lithium carbonate. Background Art

[0002] Lithium iron phosphate batteries are widely used in electric vehicles and energy storage. However, their service life is limited. After 5 to 10 years of use and possible subsequent cascade utilization, they will inevitably be recycled. Waste lithium iron phosphate (SLFP) batteries contain harmful components such as toxic electrolytes, heavy metals, plastics and binders. If not handled properly, they will cause environmental pollution. At the same time, SLFP is also a high-quality urban mineral resource containing valuable elements such as lithium, phosphorus and iron. Recycling SLFP is conducive to saving resources and protecting the environment.

[0003] There are two main methods for recycling SLFP: direct regeneration and wet recycling. Wet recycling is widely used due to its advantages of low energy consumption, mild conditions, high recovery rate, strong adaptability of raw materials and low waste gas generation. There are two main strategies for wet recycling of SLFP. One strategy is to leach most of the elements in SLFP into the solution together, then recover or remove impurity elements such as iron and phosphorus from the leachate, and finally recover lithium. This process not only consumes a lot of acid and alkali, but also causes a large loss of lithium due to co-precipitation, extraction or entrainment in the impurity removal process. Another strategy is the selective lithium leaching technology route, that is, controlling the leaching conditions to preferentially leach high-value lithium in SLFP, while most of the iron, phosphorus and other components remain in the leaching residue. Compared with the first strategy, selective lithium leaching has obvious advantages in improving the recovery rate of lithium, reducing the material consumption of the leaching process, and reducing the waste discharge of the treatment process. The key to selective lithium leaching is how to efficiently improve the selectivity of lithium leaching, that is, under the condition of obtaining the highest possible lithium leaching rate, impurity components such as iron and phosphorus enter the leachate as little as possible. In addition, during the SLFP wet lithium leaching process, a small amount of impurity components such as iron, phosphorus, fluorine and aluminum inevitably enter the leachate. In the process of purifying the lithium-containing leachate to remove the above impurities, minimizing the loss of lithium as much as possible is also crucial to improving the lithium recovery rate of the SLFP treatment process.

[0004] CN107381604A discloses a method for recovering lithium carbonate from lithium iron phosphate batteries, wherein waste lithium iron phosphate powder is placed in an inert gas environment for calcination; the calcined clinker is added with an inorganic acid and a hydrogen peroxide solution for stirring and reacting to obtain a reacted lithium iron phosphate mixed solution; the mixed solution is filtered to obtain a filtrate 1; an inorganic base is added to the filtrate 1 to adjust the pH value to 2-4, and a filtrate 2 is obtained by filtering; an inorganic base is continued to be added to the filtrate 2 to adjust the pH value to 8-11, and a filtrate 3 is obtained by filtering; the filtrate 3 is evaporated to obtain a crystal, and the crystal is sintered; water is added to the sintered product to dissolve and filter, and the filtrate is a high-concentration lithium-rich solution; a saturated carbonate solution is added dropwise to the lithium-rich solution, and after sufficient reaction, the solution is filtered, washed, precipitated, and dried to obtain lithium carbonate. The calcined lithium iron phosphate powder is leached by inorganic acid oxidation, which is not selective for lithium leaching, and the product purity cannot reach the battery level and a large lithium loss will be caused during the impurity removal process.

[0005] CN108394919A discloses the application of a metal ion complexing agent in the recycling process of waste lithium iron phosphate batteries. The waste batteries are pre-treated to obtain a black powder, which is then dissolved in a composite solution of a dilute acid and an oxidant, heated and stirred, and filtered to obtain a filtrate containing Fe and Li; a metal ion complexing agent is added to adjust the pH value, and a filtrate containing Li is separated. + The enriched solution is heated and concentrated, and then CO is introduced 3 2- , get Li 2 CO 3 Precipitation. By adding metal ion complexing agents, PO can be effectively removed. 4 3- The interference effect of Li 3 PO 4 , thereby increasing the recovered Li 2 CO 3 Purity. This method also uses inorganic acid oxidation to leach lithium iron phosphate powder, and the leaching selectivity for lithium is not high. The impurity removal process for the leachate is only applicable to environments with simple impurity components, and the lithium loss caused by the impurity removal process is not taken into account. Summary of the invention In view of the problems existing in the prior art, the first object of the present invention is to provide a method for selectively leaching black powder of lithium iron phosphate batteries. The second object of the present invention is to provide a method for recovering battery-grade lithium carbonate from black powder of lithium iron phosphate batteries.

[0006] The lithium iron phosphate battery black powder mentioned in the present invention refers to the mixed waste or positive electrode waste obtained by industrial disassembly and screening of waste lithium iron phosphate, which contains impurities such as carbon, aluminum, copper, fluorine, nickel, cobalt, and manganese in addition to phosphorus, iron, and lithium.

[0007] To achieve the above objectives, the present invention provides the following specific technical solutions.

[0008] In a first aspect, the present invention provides a method for selectively leaching black powder of a lithium iron phosphate battery, comprising: A nitric acid solution is added to the lithium iron phosphate battery black powder and leached at 105-200°C.

[0009] In a further preferred embodiment, the leaching is carried out at 105-140°C.

[0010] In a further preferred embodiment, a regulator is added during the leaching process; the regulator is a phosphorus compound or an iron compound.

[0011] Preferably, the phosphorus compound is H 3 PO 4 、Na 3 PO 4 At least one of; the iron compound is FeCl 3 、Fe(NO 3 ) 3 At least one of .

[0012] In a further preferred embodiment, the solid-liquid ratio of the added lithium iron phosphate battery black powder and the nitric acid solution is 1g:3~10mL.

[0013] In a further preferred embodiment, the HNO in the nitric acid solution is 3 The molar ratio of Li to lithium iron phosphate battery black powder is 1.3~2.2:1.

[0014] In a further preferred embodiment, the amount of the adjusting agent added is 0.5-6% of the mass of the lithium iron phosphate battery black powder.

[0015] In a further preferred embodiment, the leaching time is 0.5 to 4 hours.

[0016] In a second aspect, the present invention provides a method for recovering battery-grade lithium carbonate from lithium iron phosphate battery black powder, comprising: (1) obtaining a selective leaching solution by the aforementioned selective leaching method of lithium iron phosphate battery black powder; (2) adding a calcium-containing reagent to the selective leaching solution, and then adjusting the pH value of the selective leaching solution to 5.9-6.5 to obtain slurry I; after aging, the slurry I is subjected to solid-liquid separation to obtain a first stage of purified liquid and a first stage of impurity-removed slag; (3) The first stage purified liquid is evaporated and concentrated, and then the pH value of the first stage purified liquid is adjusted to 10-12 to obtain slurry II; after aging, the slurry II is subjected to solid-liquid separation to obtain the second stage purified liquid and the second stage impurity removal residue; (4) Deeply removing calcium from the second-stage purified liquid, then aging it, and obtaining the third-stage purified liquid and the third-stage impurity-removed slag after solid-liquid separation; (5) The three-stage purified liquid is heated, EDTA is added and stirred, and then sodium carbonate is added to precipitate crude lithium carbonate; the crude lithium carbonate is stirred and washed with hot water to obtain battery-grade lithium carbonate.

[0017] In a further preferred embodiment, the calcium-containing reagent is at least one of a calcium salt, a calcium oxide, and a calcium hydroxide. More preferably, CaCl 2 、Ca(NO 3 ) 2 、CaSO 4 , CaO. It is further preferred that the amount of calcium-containing reagent added is determined according to a molar ratio of the added Ca to the F in the selective leaching solution of 0.3-0.5:1.

[0018] In a further preferred embodiment, the three-stage washing is used to remove impurities and residues, and the washing liquid and the second-stage purification liquid are mixed before the operation of step (4).

[0019] In a further preferred embodiment, the aging temperature in step (2) is 30-50° C., and the aging time is 2-8 hours.

[0020] In a further preferred embodiment, the aging temperature in step (3) is 30-80° C., and the aging time is 2-8 hours.

[0021] In a further preferred embodiment, in step (4), calcium in the second-stage purified liquid is deeply removed by adding at least one of sodium carbonate and sodium oxalate solids to the second-stage purified liquid for deep calcium removal. It is further preferred that 2 to 12 g of sodium carbonate and / or sodium oxalate solids are added per liter of the second-stage purified liquid.

[0022] In a further preferred embodiment, the aging temperature in step (4) is 30-80° C., and the aging time is 2-8 hours.

[0023] In a further preferred embodiment, in step (5), the three-stage purified liquid is heated to 90-100°C.

[0024] In a further preferred embodiment, in step (5), 0.002-0.01 mol of EDTA is added per liter of the three-stage purification liquid.

[0025] Lithium leaching selectivity in the present invention SEL锂 according to SEL锂 = C Li / (C Li + C Fe + C P )*100% calculation, where C Li is the concentration of lithium in the leaching solution, C Feis the concentration of iron in the leaching solution, C P is the phosphorus concentration in the leachate.

[0026] The lithium loss in the present invention is based on LOS锂 = m 渣 * Li / (C Li * V)*100% calculation, where m 渣 To improve the quality of slag removal, Li To remove the lithium content in the slag, C Li is the concentration of lithium in the leachate, and V is the volume of the leachate.

[0027] Compared with the prior art, the above one or more technical solutions of the present invention can achieve at least one of the following beneficial effects: The present invention uses nitric acid at high temperature to leach black powder of lithium iron phosphate batteries, the lithium leaching rate can be as high as more than 99.5%, and the lithium leaching selectivity can be as high as more than 75%.

[0028] Further, by adding a regulator to the nitric acid high-temperature leaching system to leach the lithium iron phosphate battery black powder, the lithium leaching rate can be as high as over 99.5%, and the lithium leaching selectivity can reach over 95%.

[0029] The present invention recovers lithium carbonate from the selective leaching solution, and the lithium loss in the impurity removal process is small, and the lithium loss can be less than 0.3%. In addition, the amount of reagents used in the impurity removal process is small, and the purity of the lithium carbonate is high, reaching the standard of battery-grade lithium carbonate. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a process flow chart for recovering lithium carbonate.

[0031] Figure 2 This is the XRD diagram of the product lithium carbonate obtained in Example 6.

[0032] Figure 3 This is the SEM image of the lithium carbonate product obtained in Example 6. DETAILED DESCRIPTION

[0033] Some embodiments of the present invention provide a method for selectively leaching black powder of a lithium iron phosphate battery, comprising: A nitric acid solution is added to the lithium iron phosphate battery black powder and leached at 105-200°C.

[0034] The applicant believes that: using nitric acid to leach lithium iron phosphate battery black powder at 105-200°C, that is, high-temperature leaching under pressure, nitric acid also acts as an oxidant to oxidize iron (II) to iron (III), and iron (III) combines with phosphorus in the solution to form iron phosphate hydrate and remains in the leached residue, which can achieve selective leaching of lithium in SLFP under a simple system. The nitric acid micro-pressure high-temperature leaching system achieves lithium selective leaching of lithium from lithium iron phosphate battery black powder, which is a major innovation of the present invention. Moreover, the lithium leaching rate of lithium iron phosphate battery black powder is very high when nitric acid micro-pressure high-temperature leaching is used.

[0035] It is further preferred to carry out leaching at 105-140° C. At this temperature, the leaching rate of lithium is higher, the leaching selectivity of lithium is higher, and energy can be further saved.

[0036] Further research found that after years of recycling of lithium iron phosphate batteries, the iron-phosphorus ratio in SLFP black powder has changed. During the selective leaching process, there will be more iron or phosphorus in the leachate. Due to the lack of corresponding phosphorus or iron, iron phosphate is generated and left in the leaching residue, causing the lithium leaching selectivity to fail to reach the expected value. Based on this discovery, the present invention adds a regulator to dynamically compensate for part of the iron or phosphorus, thereby improving the lithium leaching selectivity.

[0037] In some embodiments of the present invention, a regulator is added during the leaching process; the regulator is a phosphorus compound or an iron compound. Theoretically, a phosphorus compound that can react with iron ions to form iron phosphate or an iron compound that can react with phosphorus to form iron phosphate can be used as a regulator. In a specific embodiment of the present invention, the phosphorus compound is preferably H 3 PO 4 、Na 3 PO 4 At least one of; the iron compound is FeCl 3 、Fe(NO 3 ) 3 At least one of .

[0038] In some embodiments of the present invention, the solid-liquid ratio of lithium iron phosphate battery black powder and nitric acid solution is 1g:3~10mL, for example 1:4, 1:5, 1:6, 1:8. However, it should be understood that under the technical concept of the present invention, the conventional adjustment of the leaching solid-liquid ratio by those skilled in the art according to the leaching effect is also within the protection scope of the present invention.

[0039] In some embodiments of the present invention, HNO in the nitric acid solution 3 The molar ratio of HNO to Li in the black powder of lithium iron phosphate battery is 1.3-2.2:1, for example 1.5:1, 1.6:1, 2.0:1. However, it should be understood that under the technical concept of the present invention, those skilled in the art can determine the HNO 3Conventional adjustment of the molar ratio of Li is also within the scope of the present invention.

[0040] In some embodiments of the present invention, the amount of the regulator added is 0.5-6% of the mass of the lithium iron phosphate battery black powder, such as 1% and 6%. However, it should be understood that under the technical concept of the present invention, the conventional adjustment of the amount of the regulator added by those skilled in the art according to the leaching effect is also within the protection scope of the present invention.

[0041] In some embodiments of the present invention, the leaching time is 0.5-4 hours, for example 4 hours. Those skilled in the art can adaptively adjust the leaching time according to actual leaching conditions.

[0042] Some embodiments of the present invention also provide a method for recovering battery-grade lithium carbonate from lithium iron phosphate battery black powder, comprising: (1) obtaining a selective leaching solution by the aforementioned selective leaching method of lithium iron phosphate battery black powder; (2) adding a calcium-containing reagent to the selective leaching solution, and then adjusting the pH value of the selective leaching solution to 5.9-6.5 to obtain slurry I; after aging, the slurry I is subjected to solid-liquid separation to obtain a first stage of purified liquid and a first stage of impurity-removed slag; (3) The first stage purified liquid is evaporated and concentrated, and then the pH value of the first stage purified liquid is adjusted to 10-12 to obtain slurry II; after aging, the slurry II is subjected to solid-liquid separation to obtain second stage purified liquid and second stage impurity removal residue; (4) Deeply removing calcium from the second-stage purified liquid, then aging it, and obtaining the third-stage purified liquid and the third-stage impurity-removed slag after solid-liquid separation; (5) The three-stage purified liquid is heated, EDTA is added and stirred, and then sodium carbonate is added to precipitate crude lithium carbonate; the crude lithium carbonate is stirred and washed with hot water to obtain battery-grade lithium carbonate.

[0043] The applicant found in the research process that the selective leaching solution contains F and Al. If the pH value is adjusted directly with NaOH, lithium-containing cryolite Na 3 Li 3 (AlF 6 ) 2 , resulting in chemical loss of lithium. Therefore, before adjusting the pH, some calcium ions are actively introduced, and the fluoride ions in the solution combine with calcium ions to form calcium fluoride, which avoids the formation of lithium cryolite and greatly reduces lithium loss. Then, the pH value of the selective leaching solution is adjusted to 5.9~6.5. Impurities such as Al, Cu, Fe, and P are removed at this stage, and further aging ensures that the impurities are fully precipitated. It should be noted that the pH adjustment at this stage cannot be too high, otherwise the impurities of Al and F will dissolve back into the solution; of course, the pH adjustment at this stage cannot be too low, otherwise impurities such as Cu, Al and F cannot be deeply removed.

[0044] It is inevitable that impurities such as Ni, Co, and Mn exist in the selective leaching solution. Ni, Co, and Mn impurities can only be removed under higher pH conditions. Therefore, in step (3), the pH value is adjusted to 10-12 to remove these impurities through hydroxide precipitation.

[0045] In a specific embodiment of the present invention, the calcium-containing reagent is at least one of a calcium salt, a calcium oxide, and a calcium hydroxide. In some specific embodiments, the calcium-containing reagent is preferably CaCl 2 、Ca(NO 3 ) 2 、CaSO 4 According to the lithium loss, it is further preferred that the amount of calcium-containing reagent added is determined according to the molar ratio of the added Ca to the F in the selective leaching solution being 0.3-0.5:1.

[0046] In some specific embodiments, the aging temperature in step (2) is 30-50° C., and the aging time is 2-8 hours.

[0047] In some specific implementations, in step (3), a section of the purified liquid is evaporated and concentrated to a Li concentration greater than 20 g / L.

[0048] In some specific embodiments, the aging temperature in step (3) is 30-80° C., and the aging time is 2-8 hours.

[0049] In some specific embodiments, in step (4), calcium in the second-stage purified liquid is deeply removed by adding at least one of sodium carbonate and sodium oxalate solids to the second-stage purified liquid for deep calcium removal. According to the calcium removal effect, it is further preferred to add 2 to 12 g of sodium carbonate and / or sodium oxalate solids per liter of the second-stage purified liquid.

[0050] In the process of removing impurities from the selective leaching solution, in order to prevent lithium from being lost in the form of lithium cryolite, the present invention actively introduces part of Ca, which cannot be deeply removed in the first two purification processes. If calcium is removed by generating calcium hydroxide, the pH value must be adjusted to above 14, which consumes a large amount of alkali. The present invention precipitates calcium by adding a small amount of sodium carbonate or sodium oxalate. The introduction of a small amount of carbonate and oxalate ions only causes a small amount of lithium to be co-precipitated, but this part can still be washed and dissolved, and the washing liquid can be recovered without causing lithium loss.

[0051] In some specific embodiments, the washing process is performed in three stages to remove impurities and slag, and the washing liquid and the second stage purification liquid are mixed before the operation of step (4).

[0052] In some specific embodiments, the aging temperature in step (4) is 30-80° C., and the aging time is 2-8 hours.

[0053] In the process of recovering lithium carbonate, the temperature of the leaching solution and the purification solution has little effect on the impurity removal effect, and room temperature (30°C) or higher temperatures are acceptable. From the perspective of process consistency, it is preferred to heat the leaching solution or the purification solution to the aging temperature.

[0054] In some specific embodiments, in step (5), the three-stage purified liquid is heated to 90-100°C.

[0055] In some specific embodiments, in step (5), 0.002-0.01 mol of EDTA is added to each liter of the three-stage purification solution. EDTA is added before lithium precipitation to complex various metal cations, further reducing the amount of metal impurities entering the lithium carbonate product during the lithium precipitation process.

[0056] In the specific implementation process, stirring is performed during the impurity removal process of step (2), step (3), step (4), and step (5). An appropriate stirring speed is adjusted to avoid excessive local concentration of the impurity removal agent, which affects the impurity removal effect. In a specific embodiment, the preferred stirring speed is 200-800 rpm, such as 200 rpm, 400 rpm, 600 rpm, and 800 rpm. Of course, those skilled in the art can also adjust the stirring speed according to actual conditions.

[0057] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0058] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0059] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0060] Example 1 The composition of SLFP (wt.%) is: Li: 3.18%, Fe: 25.23%, P: 16.20%, C: 15.98%, Al: 0.58%, Cu: 1.58%, F: 2.81%, Ni: 0.76%, Co: 0.31%, Mn: 0.44%.

[0061] Leaching: (1) Leachate-solid ratio: L / S = 8 (2) Leaching reagent: nitric acid solution. The amount of nitric acid solution added is based on HNO 3 The / Li molar ratio was determined to be 2.0.

[0062] (3) Leaching environment: closed environment (4) Leaching temperature: 120℃ (5) Leaching time: 4h After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 1.

[0063] Table 1 The lithium leaching rate is: 99.56%.

[0064] The leaching selectivity of lithium is: 78.44%.

[0065] Example 2 The only difference between Example 2 and Example 1 is that the leaching temperature is 105° C. and the leaching liquid-to-solid ratio L / S is 5.

[0066] After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 2.

[0067] Table 2 The lithium leaching rate is: 99.51%.

[0068] The leaching selectivity of lithium is: 75.13%.

[0069] Example 3 The only difference between Example 3 and Example 1 is that the leaching temperature is 200° C. and the leaching liquid-to-solid ratio L / S is 10.

[0070] After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 3.

[0071] Table 3 The lithium leaching rate is: 96.34%.

[0072] The leaching selectivity of lithium is: 71.03%.

[0073] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is that the leaching temperature is 90°C.

[0074] After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 4.

[0075] Table 4 The lithium leaching rate is: 99.66%.

[0076] The leaching selectivity of lithium is: 10.81%.

[0077] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that the leaching temperature is 100°C.

[0078] After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 5.

[0079] Table 5 The lithium leaching rate is: 99.60%.

[0080] The leaching selectivity of lithium is: 17.32%.

[0081] Example 4 The composition of SLFP (wt.%) is: Li: 3.18%, Fe: 25.23%, P: 16.20%, C: 15.98%, Al: 0.58%, Cu: 1.58%, F: 2.81%, Ni: 0.76%, Co: 0.31%, Mn: 0.44%.

[0082] Leaching: (1) Leaching system: HNO 3 +Fe(NO 3 ) 3 , the leaching liquid-solid ratio L / S = 8, the amount of nitric acid solution added is based on HNO 3 / Li molar ratio is determined to be 2.0, and the adjusting agent Fe(NO 3 ) 3 The added amount is 6.0 wt% of the black powder mass.

[0083] (2) Leaching temperature: 120℃ (3) Leaching environment: closed environment (4) Leaching time: 4h.

[0084] After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 6.

[0085] Table 6 The lithium leaching rate is: 99.65%.

[0086] The leaching selectivity of lithium is: 95.42%.

[0087] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that: HNO 3 and Fe(NO 3 ) 3The timing of joining is different.

[0088] Specifically: Leaching: (1) Leaching system: HNO 3 , the leaching liquid-solid ratio L / S = 8, the amount of nitric acid solution added is based on HNO 3 The / Li molar ratio was determined to be 2.0.

[0089] (2) Leaching temperature: 120℃ (3) Leaching environment: closed environment (4) Leaching time: 4h.

[0090] After leaching is completed, the solid and liquid are separated to obtain leachate I.

[0091] The leaching solution I was cooled to room temperature, and then 6.0 wt% of the black powder mass of the adjusting agent Fe(NO 3 ) 3 After the reaction is completed, the solid and liquid are separated to obtain leachate II.

[0092] The composition of the leaching solution II was analyzed and the results are shown in Table 7.

[0093] Table 7 The lithium leaching rate is: 99.59%.

[0094] The leaching selectivity of lithium is: 58.75%.

[0095] Comparative Example 4 The difference between Comparative Example 4 and Comparative Example 3 is that the leachate I and the adjusting agent react at 120° C., and after the reaction is completed, the solid and liquid are separated to obtain leachate II.

[0096] The composition of the leaching solution II was analyzed and the results are shown in Table 8.

[0097] Table 8 The lithium leaching rate is: 99.67%.

[0098] The leaching selectivity of lithium is: 83.19%.

[0099] Comparative Example 5 The difference between Comparative Example 5 and Example 3 is that the leaching temperature is 95°C.

[0100] After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 9.

[0101] Table 9 The lithium leaching rate is: 99.61%.

[0102] The leaching selectivity of lithium is: 13.33%.

[0103] Example 5 The composition of SLFP (wt.%) is: Li: 2.79%, Fe: 21.97%, P: 11.35%, C: 22.13%, Al: 0.88%, Cu: 0.58%, F: 2.11%, Ni: 0.28%, Co: 0.13%, Mn: 0.41%.

[0104] Leaching: (1) Leaching system: HNO 3 , the leaching liquid-solid ratio L / S = 6, the amount of nitric acid solution added is based on HNO 3 The / Li molar ratio was determined to be 1.6.

[0105] (2) Leaching temperature: 110℃ (3) Leaching environment: closed environment (4) Leaching time: 4h.

[0106] After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 10.

[0107] Table 10 The lithium leaching rate is: 99.60%.

[0108] The leaching selectivity of lithium is: 79.01%.

[0109] Example 6 The composition of SLFP (wt.%) is: Li: 2.79%, Fe: 21.97%, P: 11.35%, C: 22.13%, Al: 0.88%, Cu: 0.58%, F: 2.11%, Ni: 0.28%, Co: 0.13%, Mn: 0.41%.

[0110] Leaching: (1) Leaching system: HNO 3 + H 3 PO 4 , the leaching liquid-solid ratio L / S = 6, the amount of nitric acid solution added is based on HNO 3 / Li molar ratio is determined to be 1.6, and the adjusting agent H 3 PO 4 The amount added is 1.0 wt% of the black powder mass.

[0111] (2) Leaching temperature: 110℃ (3) Leaching environment: closed environment (4) Leaching time: 4h.

[0112] After leaching, the solid and liquid were separated and the composition of the leaching solution was analyzed. The results are shown in Table 11.

[0113] Table 11 The lithium leaching rate is: 99.57%.

[0114] The leaching selectivity of lithium is: 96.26%.

[0115] Comparative Example 6 The difference between Comparative Example 6 and Example 6 is that: HNO 3 and H 3 PO 4 The timing of joining is different. Specifically: Leaching: (1) Leaching system: HNO 3 The leaching liquid-solid ratio L / S = 6, the amount of nitric acid solution added is based on HNO 3 The / Li molar ratio was determined to be 1.6.

[0116] (2) Leaching temperature: 110℃ (3) Leaching environment: closed environment (4) Leaching time: 4h.

[0117] After leaching, solid and liquid were separated to obtain leachate I. 1.0 wt% of the black powder mass of the adjusting agent H was added to leachate I. 3 PO 4 , react at 110℃, and after the reaction is completed, separate the solid and liquid to obtain leachate II.

[0118] The composition of leachate II was analyzed and the results are shown in Table 12.

[0119] Table 11 The lithium leaching rate is: 99.65%.

[0120] The leaching selectivity of lithium is: 88.53%.

[0121] Comparative Example 7 The difference between Comparative Example 7 and Example 6 is that the leaching temperature is 50°C.

[0122] After leaching, the solid and liquid were separated and the composition of the leaching liquid was analyzed. The results are shown in Table 13.

[0123] Table 13 The leaching rate of lithium is: 92.04%.

[0124] The leaching selectivity of lithium is: 8.89%.

[0125] Example 7 The leachate obtained in Example 1 was used as the treatment object.

[0126] (1) Stir the 50°C leaching solution at a speed of 500 rpm, add CaO, and the amount of CaO added is determined based on the Ca / F molar ratio of 0.4. Continue stirring for 40 minutes after addition, and then add 10 mol / L NaOH solution to adjust the pH value to 6.2±0.1. Aging the slurry at 30°C for 6 hours. After aging, the solid and liquid are separated to obtain a purified liquid and a decontaminated slag.

[0127] Analysis of the first stage of impurity removal slag showed a lithium loss of 0.17%.

[0128] (2) Evaporate the first-stage purified liquid to a lithium concentration of 20±2 g / L, stir the first-stage purified liquid at 50°C at a speed of 400 rpm, add 10 mol / L NaOH solution to adjust the pH value to be stable at 11.0±0.2. Aging the slurry at 50°C for 8 hours. After aging, separate the solid and liquid to obtain the second-stage purified liquid and the second-stage impurity removal slag.

[0129] Analysis of the second-stage impurity removal slag showed a lithium loss of 0.01%.

[0130] (3) Stir the second-stage purification liquid at 60°C at a speed of 400 rpm and add 6 g of Na per liter of the second-stage purification liquid. 2 CO 3 The solid was deeply decalcified, and after stirring for 6 hours, the slurry was aged at 60°C for 8 hours, and then the solid-liquid was separated to obtain three-stage purified liquid and three-stage impurity-removed slag.

[0131] (4) Heat the three-stage purification liquid to 95±2℃, then add 0.008 mol of EDTA per liter of the three-stage purification liquid, stir and react for 0.5h, and then add 2.5 mol / L of Na 2 CO 3 The solution is used to precipitate crude lithium carbonate.

[0132] (5) Washing the crude lithium carbonate with hot water to obtain product lithium carbonate.

[0133] The contents of various components in the product lithium carbonate are shown in Table 14.

[0134] Table 14 Lithium carbonate content (wt.%) Figure 2This is the XRD diagram of the product lithium carbonate.

[0135] Figure 3 This is the SEM image of the lithium carbonate product.

[0136] Comparative Example 8 The only difference between Comparative Example 8 and Example 7 is that no CaO is added in step (1), and the pH value is directly adjusted to remove impurities.

[0137] That is, step (1) is: The leaching solution at 50°C was stirred at a speed of 500 rpm, and a 10 mol / L NaOH solution was added to adjust the pH value to be stable at 6.2±0.1. The slurry was aged at 30°C for 6 hours. After the aging was completed, the solid and liquid were separated to obtain a purified liquid and a decontaminated slag.

[0138] Analysis of the first stage of impurity removal slag showed a lithium loss of 2.61%.

[0139] Steps (2), (3), (4) and (5) are the same as those in Example 7.

[0140] Analysis of the second-stage impurity removal slag showed a lithium loss of 0.01%.

[0141] Example 8 The leachate obtained in Example 4 was used as the treatment object.

[0142] (1) Stir the leaching solution at 30°C at 800 rpm and add Ca(NO 3 ) 2 , Ca(NO 3 ) 2 The amount of addition is determined based on the Ca / F molar ratio of 0.3. After addition, stirring is continued for 20 minutes, and then 10 mol / L NaOH solution is added to adjust the pH value to be stable at 6.0±0.1. The slurry is aged at 30°C for 2 hours. After aging, the solid and liquid are separated to obtain a purified liquid and a decontaminated slag.

[0143] Analysis of the first stage of impurity removal slag showed a lithium loss of 0.26%.

[0144] (2) Evaporate the first-stage purified liquid to a lithium concentration of 20±2 g / L, stir the first-stage purified liquid at 400 rpm at 30°C, add 10 mol / L NaOH solution to adjust the pH value to 10.5±0.2. Aging the slurry at 30°C for 4 hours. After aging, separate the solid and liquid to obtain the second-stage purified liquid and the second-stage impurity removal slag.

[0145] Analysis of the second-stage impurity removal slag showed a lithium loss of 0.01%.

[0146] (3) The second-stage purified liquid at 30°C was stirred at a rotation speed of 400 rpm, and 12 g of sodium oxalate solid was added per liter of the second-stage purified liquid for deep decalcification. After stirring for 4 hours, the slurry was aged at 30°C for 8 hours, and then the solid-liquid was separated to obtain the third-stage purified liquid and the third-stage impurity-removed slag.

[0147] (4) Heat the three-stage purification solution to 95±2℃, then add 0.01 mol EDTA per liter of the three-stage essence solution, stir and react for 0.5h, and then add Na2SO4 at a concentration of 2.5 mol / L according to the amount of lithium in the three-stage purification solution and the lithium precipitation effect. 2 CO 3 The solution is used to precipitate crude lithium carbonate.

[0148] (5) Washing the crude lithium carbonate with hot water to obtain product lithium carbonate.

[0149] The contents of various components in the product lithium carbonate are shown in Table 15.

[0150] Table 15 Lithium carbonate content (wt.%) Example 9 The leachate obtained in Example 6 was used as the treatment object.

[0151] (1) Stir the 50°C leaching solution at 600 rpm and add CaCl 2 , CaCl 2 The amount of addition is determined based on the Ca / F molar ratio of 0.5. After addition, stirring is continued for 60 minutes, and then 8 mol / L NaOH solution is added to adjust the pH value to be stable at 6.4±0.1. The slurry is aged at 50°C for 6 hours. After aging, the solid and liquid are separated to obtain a purified liquid and a decontaminated slag.

[0152] Analysis of the first stage of impurity removal slag showed a lithium loss of 0.13%.

[0153] (2) Evaporate the first-stage purified liquid to a lithium concentration of 24±2 g / L, stir the first-stage purified liquid at 80°C at a speed of 200 rpm, add 8 mol / L NaOH solution to adjust the pH value to be stable at 11.5±0.2. Aged the slurry at 80°C for 2 h. After aging, separate the solid and liquid to obtain the second-stage purified liquid and the second-stage impurity removal slag.

[0154] Analysis of the second-stage impurity removal slag showed a lithium loss of 0.01%.

[0155] (3) The second-stage purified liquid was stirred at 80°C at a rotation speed of 200 rpm, and 2 g of sodium carbonate solid was added per liter of the second-stage purified liquid for deep decalcification. After stirring for 10 hours, the slurry was aged at 80°C for 2 hours, and then the solid-liquid was separated to obtain the third-stage purified liquid and the third-stage impurity-removed slag.

[0156] (4) Heat the three-stage purification liquid to 95±2℃, then add 0.002 mol of EDTA per liter of the three-stage purification liquid, stir and react for 1 hour, and then add 2.5 mol / L of Na 2 CO 3 The solution is used to precipitate crude lithium carbonate.

[0157] (5) Washing the crude lithium carbonate with hot water to obtain product lithium carbonate.

[0158] The contents of various components in the product lithium carbonate are shown in Table 16.

[0159] Table 16 Lithium carbonate content (wt.%) The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A selective leaching method for black powder of lithium iron phosphate battery, It is characterized in that include: A nitric acid solution is added to the lithium iron phosphate battery black powder and leached at 105-200°C.

2. The selective leaching method of lithium iron phosphate battery black powder according to claim 1, It is characterized in that A regulator is added during the leaching process; the regulator is a phosphorus compound or an iron compound.

3. The selective leaching method of lithium iron phosphate battery black powder as claimed in claim 2, It is characterized in that The phosphorus compound is H 3 PO 4 、Na 3 PO 4 At least one of; the iron compound is FeCl 3 、Fe(NO 3 ) 3 At least one of .

4. The selective leaching method for lithium iron phosphate battery black powder according to any one of claims 1 to 3, It is characterized in that The solid-liquid ratio of lithium iron phosphate battery black powder and nitric acid solution is 1g:3~10mL; Preferably, the HNO in the nitric acid solution is 3 The molar ratio of Li to lithium iron phosphate battery black powder is 1.3~2.2:

1.

5. The selective leaching method of lithium iron phosphate battery black powder as claimed in claim 2 or 3, It is characterized in that The amount of the adjusting agent added is 0.5-6% of the mass of the lithium iron phosphate battery black powder.

6. Method for recovering battery-grade lithium carbonate from lithium iron phosphate battery black powder, It is characterized in that include: (1) Obtaining a selective leaching solution by the selective leaching method for lithium iron phosphate battery black powder according to any one of claims 1 to 5; (2) adding a calcium-containing reagent to the selective leaching solution, and then adjusting the pH value of the selective leaching solution to 5.9-6.5 to obtain slurry I; after aging, the slurry I is subjected to solid-liquid separation to obtain a first stage of purified liquid and a first stage of impurity-removed slag; (3) evaporating and concentrating the first stage purified liquid, and then adjusting the pH value of the first stage purified liquid to 10-12 to obtain slurry II; After aging, the slurry II is subjected to solid-liquid separation to obtain the second-stage purified liquid and the second-stage impurity-removed slag; (4) Deeply removing calcium from the second-stage purified liquid, then aging it, and obtaining the third-stage purified liquid and the third-stage impurity-removed slag after solid-liquid separation; (5) The three-stage purified liquid is heated, EDTA is added and stirred, and sodium carbonate is added to precipitate crude lithium carbonate; the crude lithium carbonate is stirred and washed with hot water to obtain battery-grade lithium carbonate.

7. The method for recovering battery-grade lithium carbonate from lithium iron phosphate battery black powder as claimed in claim 6, It is characterized in that The calcium-containing reagent is at least one of a calcium salt, a calcium oxide, and a calcium hydroxide; Preferably, the calcium-containing reagent is CaCl 2 、Ca(NO 3 ) 2 、CaSO 4 , CaO; Preferably, the amount of the calcium-containing reagent added is determined based on a molar ratio of 0.3 to 0.5:1 between the added Ca and the F in the selective leaching solution.

8. The method for recovering battery-grade lithium carbonate from lithium iron phosphate battery black powder as claimed in claim 6 or 7, It is characterized in that The aging temperature in step (2) is 30-50° C. and the aging time is 2-8 hours; Preferably, the aging temperature in step (3) is 30-80° C., and the aging time is 2-8 hours; Preferably, the aging temperature in step (4) is 30-80° C., and the aging time is 2-8 hours.

9. The method for recovering battery-grade lithium carbonate from lithium iron phosphate battery black powder as claimed in claim 6 or 7, It is characterized in that In step (4), calcium in the second-stage purified liquid is deeply removed by: adding at least one of sodium carbonate and sodium oxalate solids to the second-stage purified liquid for deep calcium removal; Preferably, 2-12 g of sodium carbonate and / or sodium oxalate solid is added to each liter of the second-stage purified liquid.

10. The method for recovering battery-grade lithium carbonate from lithium iron phosphate battery black powder as claimed in claim 6 or 7, It is characterized in that In step (5), the three-stage purified liquid is heated to 90-100°C; Preferably, in step (5), 0.002-0.01 mol of EDTA is added per liter of the three-stage purification liquid.

Citation Information

Patent Citations

  • Method for recycling lithium carbonate from lithium iron phosphate battery

    CN107381604A

  • Application of metal ion complexing agent in waste and old lithium iron phosphate battery recovery process

    CN108394919A

Cited By

  • Recycling method of lithium iron phosphate black powder

    CN119637912A

  • Method for selectively leaching lithium from mixed black powder of positive electrode and negative electrode of waste lithium ion battery