Process for preparing anhydrous rare earth fluoride from rare earth reducing slag by one-step method

Anhydrous fluorinated rare earths were prepared from rare earth reduction slag by one-step hydrothermal method, which solved the equipment corrosion and pollution problems caused by high-temperature roasting transformation in the existing technology, and achieved efficient recycling and recycling of rare earth and fluorine resources.

CN119040641AActive Publication Date: 2024-11-29JIANGXI IONIC RARE EARTH ENG RES CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411155796.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

When the prior art recovers rare earths and fluorine elements from rare earth reduction slag, a high-temperature roasting transformation process is required, resulting in high corrosiveness of the equipment and serious pollution of hydrogen fluoride gas, which increases the difficulty of rare earth purification, long process flow and low rare earth yield.

Method used

The rare earth and fluorine in the rare earth reduction slag are directly prepared into fluorinated rare earths through one-step hydrothermal method. Anhydrous fluorinated rare earths are obtained through washing, vacuum heating and roasting processes, realizing the recycling and recycling of rare earths and fluorine resources.

Benefits of technology

The process flow has been simplified, the recovery rate of rare earth and fluorine resources has been improved to more than 96%, avoiding the pollution of hydrogen fluoride waste gas during the high-temperature transformation, and achieving green and efficient recycling of rare earth reduction slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040641A_ABST
    Figure CN119040641A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of industrial waste residue treatment, in particular to a process for preparing anhydrous rare earth fluoride from rare earth reducing slag through a one-step method. The method provided by the invention comprises the following steps: carrying out crushing, ball milling, acidification and other treatments on a rare earth reducing slag raw material, carrying out a precipitation conversion reaction on the treated slag and a rare earth chloride feed liquid, filtering to obtain rare earth fluoride and a filtrate, and carrying out filtering, washing, drying, vacuum roasting and other processes on the generated rare earth fluoride to prepare anhydrous rare earth fluoride. And enriching rare earth chloride and calcium chloride in the filtrate by using a P507 extracting agent, and returning for reutilization. According to the technology, rare earth and fluorine in the rare earth reducing slag are synchronously converted through a one-step hydrothermal method, resource recycling of the rare earth and the fluorine is achieved, the technological process is simple, and industrial production is easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of industrial waste residue treatment, and in particular to a process for preparing anhydrous rare earth fluoride from rare earth reduction residue in one step while recovering rare earth and fluorine elements. Background Art

[0002] In the production of high melting point rare earth metals (such as Gd, Tb, Dy, Ho, Er, Y, Lu metals, Tb-Dy alloys, etc.), metallic calcium is generally used as a reducing agent and rare earth fluorides are used as raw materials. Rare earth metals are generated under high temperature conditions, and calcium thermal reduction slag is also produced. The main component of the slag is calcium fluoride. Some rare earth fragments and incompletely converted materials also enter the calcium fluoride slag. The rare earth (REO) content is usually 0.9-8%, mainly rare earth metals, rare earth oxides, rare earth fluorides, fluoride oxides, etc.

[0003] In recent years, invention patents have been developed for recovering valuable elements such as rare earths and fluorine from reduced slag through methods such as magnetic separation-sulfuric acid transformation, sodium silicate roasting transformation, and lithium salt vacuum roasting transformation. For example, in Chinese invention patent CN 116287735A, calcium-terbium waste residue is converted into powder by fully drying in the air, and terbium rare earth concentrate and calcium fluoride are selected by a magnetic separator. Rare earth oxides are obtained by sulfuric acid acidification, oxalic acid precipitation, calcination and other processes; in Chinese invention patent CN 105177324 B, sodium silicate and vacuum calcium thermal reduction rare earth residue powder are subjected to high-temperature roasting and hydrochloric acid acidification to separate rare earth liquid; in Chinese invention patent CN111961872 A, lithium salt is mixed with calcium thermal reduction residue and then vacuum replaced, and then vacuum distilled to obtain high-purity lithium fluoride, and the distillation residue is then subjected to acid leaching, extraction, precipitation, calcination and other processes to obtain rare earth oxides; in Chinese invention patent CN 116497241B, lithium carbonate is mixed with terbium calcium residue and then roasted, and the roasted mixture is immersed in a leaching solution for leaching and solid-liquid separation to obtain a mixture of terbium oxide and lithium fluoride. All of these schemes require the use of a high-temperature roasting transformation process to decompose rare earth fluoride and calcium fluoride. However, fluorine-containing compounds and high-acid treatment conditions are highly corrosive to equipment, and the resulting hydrogen fluoride gas causes serious pollution to the environment. At the same time, other elements need to be introduced into the transformation process, which increases the difficulty of rare earth purification. The product obtained is mainly a rare earth chloride solution, which needs to be further extracted, precipitated, and burned to obtain an oxide rare earth product. The process is long and the rare earth yield is low. Summary of the invention

[0004] In view of this, the present invention provides a one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag, and adopts a hydrothermal method to directly prepare rare earth fluoride from rare earth reduction slag, thereby realizing the recovery and recycling of rare earth and fluorine resources. The rare earth fluoride is washed to remove impurities, and then vacuum heated to obtain anhydrous rare earth fluoride, which is returned for use as a raw material for calcium thermal reduction. The present invention can recycle calcium, fluorine and rare earth elements in rare earth reduction slag, reducing resource waste and production costs.

[0005] The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag proposed by the present invention comprises:

[0006] Step 1: The blocky rare earth reduction slag is crushed and ball-milled into powder;

[0007] Step 2: Mix the powder obtained in step 1 with pure water, remove the generated gas under stirring, and obtain a supernatant and water-leached residue after standing. The water-leached residue is further subjected to acidification, filtration, and water washing to obtain treated rare earth reduction residue;

[0008] Step 3: The treated rare earth reduction slag obtained in step 2 is mixed with the same type of rare earth chloride feed liquid, the mixed slurry is placed in a high-pressure reactor, a sealing cover is put on, stirring is started, a precipitation conversion reaction is carried out under high temperature conditions, and rare earth fluoride and filtrate are obtained by filtering;

[0009] Step 4: The rare earth fluoride obtained in step 3 is subjected to washing, drying, vacuuming and roasting processes to obtain anhydrous rare earth fluoride;

[0010] Step 5: The filtrate obtained in step 3 contains rare earth chloride and calcium chloride. The rare earth is enriched using P507 extractant and returned to step 3 for recycling.

[0011] Preferably, the rare earth reduction slag in step 1 includes one or more of metal terbium reduction slag, metal dysprosium reduction slag, metal yttrium reduction slag, and metal gadolinium reduction slag.

[0012] Preferably, the composition of the rare earth reduction slag in step 1 includes Ca: 45-57%, F: 40%-49%, RE: 0.6%-10%.

[0013] Preferably, in step 2, the mass ratio of rare earth reduction slag powder to pure water is 1:3-10, and the stirring speed is 100-160 r / min.

[0014] Preferably, in step 2, 0.5-3 mol / L hydrochloric acid is used for acidification, the pH of the solution after acidification is 0.5-1.5, and after filtration, it is washed with pure water, and the acid water obtained by filtration is neutralized with the supernatant.

[0015] Preferably, in step three, the concentration of the rare earth chloride solution is 1.0 mol / L to 1.5 mol / L, the pH of the rare earth solution is adjusted to 1 to 4 using ammonium bicarbonate, the amount of rare earth reduction slag input and the amount of rare earth solution input are calculated according to the molar ratio of fluorine in the rare earth reduction slag to REO in the rare earth solution, and the molar ratio of fluorine in the rare earth reduction slag to REO in the rare earth solution is 3:1.0 to 3.0.

[0016] Preferably, in step three, the precipitation conversion reaction temperature is 90-200° C., the stirring speed is 150-300 r / min, and the reaction time is 200-300 min.

[0017] Preferably, in the step 4, pure water is used for washing, and the mass ratio of rare earth fluoride to pure water is 1:50-70. The washed rare earth fluoride is dried at a drying temperature of 100-110°C and a drying time of 180-480 min. After drying, vacuum is drawn to a vacuum degree of minus 50 kPa to minus 20 kPa, and the vacuum is turned off for roasting at a temperature of 600-800°C for a time of 120-360 min.

[0018] The beneficial effects achieved by the present invention are as follows:

[0019] (1) The same type of rare earth chloride liquid in the reducing slag is used to realize the transformation and decomposition of rare earth and calcium fluoride in the reducing slag under a hydrothermal system, and rare earth fluoride is prepared in one step. The process is simple and easy to operate; (2) The invention simultaneously realizes the comprehensive recovery of rare earth and fluorine resources in the reducing slag, and the recovery rate reaches more than 96%; (3) The inventive process realizes the recovery of rare earth and fluorine resources in aqueous solution, avoiding the pollution of waste gas such as hydrogen fluoride and chlorine generated in the high-temperature transformation process, and at the same time does not produce fluorine-containing wastewater, thereby realizing green and efficient recovery of reducing slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention is a schematic flow chart of a one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag. DETAILED DESCRIPTION

[0021] The present invention provides a rare earth reduction slag recovery and treatment method, comprising the following steps:

[0022] Step 1: The blocky rare earth reduction slag is crushed and ball-milled into powder;

[0023] Step 2: Mix the powder obtained in step 1 with pure water, remove the generated gas under stirring, and obtain a supernatant and water-leached residue after standing. The water-leached residue is further subjected to acidification, filtration, and water washing to obtain treated rare earth reduction residue;

[0024] Step 3: The treated rare earth reduction slag obtained in step 2 is mixed with the same type of rare earth chloride feed liquid, the mixed slurry is placed in a high-pressure reactor, a sealing cover is put on, stirring is started, a precipitation conversion reaction is carried out under high temperature conditions, and rare earth fluoride and filtrate are obtained by filtering;

[0025] Step 4: The rare earth fluoride obtained in step 3 is subjected to washing, drying, vacuuming and roasting processes to obtain anhydrous rare earth fluoride;

[0026] Step 5: The filtrate obtained in step 3 contains rare earth chloride and calcium chloride. The rare earth is enriched using P507 extractant and returned to step 3 for recycling.

[0027] In the present invention, the mass percentage of calcium in the rare earth reduction slag is preferably 48-55%; the mass percentage of fluorine in the rare earth reduction slag is preferably 43-48%; the mass percentage of rare earth in the rare earth reduction slag is preferably 2-8%.

[0028] In the present invention, the blocky rare earth reduction slag is crushed by a jaw crusher, and the ball milling is performed by a wet rolling ball mill.

[0029] In the present invention, the powder is mixed with pure water, and the purpose of the mixing is to convert the metal calcium, calcium oxide and other substances remaining in the powder into calcium hydroxide and release the generated hydrogen with water molecules. In the present invention, the mass ratio of the rare earth waste to pure water is preferably 1:4-8. In the present invention, the mixing is preferably carried out under stirring conditions, and the stirring speed is preferably 120-160r / min.

[0030] After obtaining the water-leached residue, the present invention drips a hydrochloric acid solution into the water-leached residue. The molar concentration of the hydrochloric acid solution is preferably 1 to 2 mol / L. In the present invention, the pH value of the acidification is preferably 1.0 to 1.5. The acidified water-leached residue is filtered for solid-liquid separation, and the separated solid is filtered and washed with pure water. When the pH value of the washing water is preferably 6 to 7, the washing is stopped and vacuum filtration is performed.

[0031] In the present invention, the molar concentration of the rare earth solution is preferably 1.2 mol / L to 1.5 mol / L. In the present invention, the acid value of the rare earth solution is adjusted using analytically pure ammonium bicarbonate, and the adjusted pH value is preferably 2 to 3.

[0032] In the present invention, the treated rare earth reduction slag is mixed with a rare earth liquid, and the molar ratio of the mixture is preferably 3:1.2-2.8. The mixed slurry is placed in a high-pressure reactor, covered with a sealing cover, and stirred. The stirring speed is preferably 180-260 r / min. The reaction is carried out at a high temperature, and the reaction temperature is preferably 180-200°C for precipitation conversion reaction to generate rare earth fluoride.

[0033] In the present invention, after the precipitation conversion reaction, it is preferred to further include: filtering the precipitation conversion reaction system to obtain a solid. The present invention has no special requirements for the filtration, and a conventional filtration method in the art can be used. The present invention preferably washes the filter residue obtained by filtration to remove calcium ions and chloride ions on the surface. In the present invention, the washing solvent is preferably pure water. In the present invention, the mass ratio of the rare earth fluoride to pure water is preferably 1:55 to 65.

[0034] In the present invention, the drying temperature is preferably 100-105° C.; the drying time is preferably 240-420 min.

[0035] In the present invention, the calcination temperature is preferably 700-800° C.; the calcination time is preferably 3-6 hours.

[0036] In the present invention, the filtrate obtained by filtration contains a large amount of calcium chloride solution and a small amount of rare earth. In the present invention, the extraction uses P507 extractant. Calcium ions and rare earth ions are separated, and the recovered rare earth ions can be used as raw materials to achieve resource recycling.

[0037] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0038] Example 1

[0039] according to Figure 1 Anhydrous terbium fluoride is prepared in one step from metallic terbium reduction slag.

[0040] The composition of the terbium metal reduction slag is shown in Table 1.

[0041] Table 1 Composition of terbium metal reduction slag

[0042] Element RE F Ca Mass percentage (%) 5.90 46.50 47.60

[0043] Take 1.0kg of metallic terbium reduction slag and crush it with a jaw crusher. After crushing, place it in a ball mill for ball milling. Pour the ball-milled material into a 5L plastic measuring cup and mix it with 3L pure water. After mixing, obtain the supernatant and water-leached slag. Slowly add 3mol / L hydrochloric acid dropwise into the water-leached slag slurry. When the slurry is adjusted to a pH value of 1.0, stop adding hydrochloric acid, perform solid-liquid separation, and set the stirring speed to 130r / min. The separated solid (calculated as fluorine in the metallic terbium reduction slag) is mixed with 1.2 mol / L terbium chloride feed liquid (REO) in a molar ratio of 3:1.2, and the mixed slurry is placed in a 10L high-pressure reactor, covered with a sealing cover, and stirred, and a precipitation conversion reaction is carried out under high temperature conditions. The acid value of the feed liquid is adjusted to pH 3 using ammonium bicarbonate, the reaction time is controlled to 280 min, the stirring speed is 180 r / min, the reaction temperature is controlled to 180° C., and a filtration method is used for solid-liquid separation. The separated fluoride is washed with pure water, and the washing mass ratio is 1:55. The washed fluoride is dried at 105° C. for 240 min. After drying, vacuum is evacuated until the vacuum degree reaches minus 30 kPa, and vacuum is stopped. Heating is continued. When the temperature reaches 700° C., it is kept warm for 120 min. The central particle size of the generated fluoride is 4.65 um, O is 0.036%, Ca is 0.2%, and the conversion rate of fluorine reaches 99.28%. Excess terbium chloride and calcium chloride mixed solution is extracted by fractionation of organic phase with P507: kerosene-2:1 to separate metallic terbium from calcium chloride, and the enriched and separated terbium liquid is used as raw material to ensure that the rare earth liquid and rare earth reduction slag can be recovered. The organic phase washing water is neutralized with the soaking liquid of the reduction slag and pure water (i.e., the supernatant), and there is no wastewater discharge in the whole process.

[0044] Table 2 Particle size distribution data of anhydrous terbium fluoride crystals prepared in Example 1

[0045]

[0046]

[0047] Example 2

[0048] according to Figure 1 Anhydrous terbium fluoride is prepared in one step from metallic terbium reduction slag.

[0049] The composition of the terbium metal reduction slag is shown in Table 3.

[0050] Table 3 Composition of terbium metal reduction slag

[0051] Element RE F Ca Mass percentage (%) 0.85 43.90 55.25

[0052] Take 1.0kg of metallic terbium reduction slag and crush it with a jaw crusher. After crushing, place it in a ball mill for ball milling. Pour the ball-milled material into a 10L plastic measuring cup and mix it with 5L of pure water. After mixing, obtain the supernatant and water-leached slag. Slowly add 2mol / L hydrochloric acid dropwise into the water-leached slag slurry. When the slurry is adjusted to a pH value of 1.5, stop adding hydrochloric acid, perform solid-liquid separation, and set the stirring speed to 150r / min. The separated solid (in terms of fluorine in the metallic terbium reduction slag) is mixed with 1.3 mol / L terbium chloride feed liquid (REO) in a molar ratio of 3:1.6, and the mixed slurry is placed in a 20L high-pressure reactor, covered with a sealing cover, and stirred, and a precipitation conversion reaction is carried out under high temperature conditions. The acid value of the feed liquid is adjusted to a pH of 2 using analytically pure ammonium bicarbonate, the reaction time is controlled to be 290 min, the stirring speed is 200 r / min, the reaction temperature is controlled to be 190° C., and a filtration method is used for solid-liquid separation. The separated fluoride is washed with pure water, and the washing mass ratio is 1:58. The washed fluoride is dried at 103° C. for 300 min. After drying, vacuum is evacuated until the vacuum degree reaches minus 40 kPa, and vacuum is stopped. Heating is continued. When the temperature reaches 750° C., the temperature is kept for 180 min. The central particle size of the generated fluoride is 1.67 um, O is 0.048%, Ca is 0.27%, and the conversion rate of fluorine reaches 99.03%. Excess terbium chloride and calcium chloride mixed solution is fractionated and extracted by P507: kerosene-2:1 organic phase to separate metallic terbium from calcium chloride. The separated terbium liquid is used as raw material to ensure that the rare earth liquid and rare earth reduction slag can be recovered. The reduction slag acidified water and organic phase washing water are neutralized with the reduction slag and pure water soaking liquid, and there is no wastewater discharge in the whole process.

[0053] It can be seen from Examples 1 and 2 that the particle size of the generated anhydrous terbium fluoride can be adjusted by controlling the parameters to meet different particle size requirements.

[0054] Table 4 Particle size distribution data of anhydrous terbium fluoride crystals prepared in Example 2

[0055] project result <![CDATA[D 10 / μm]]> 0.74 <![CDATA[D 25 / μm]]> 1.04 <![CDATA[D 50 / μm]]> 1.67 <![CDATA[D 75 / μm]]> 2.67 <![CDATA[D 90 / μm]]> 3.79 <![CDATA[D 97 / μm]]> 5.10 <![CDATA[D 100 / μm]]> 11.18 <![CDATA[D (3,2) / μm]]> 1.38 <![CDATA[D (4,3) / μm]]> 2.01 Span 1.83 <![CDATA[Specific surface area by weight / m 2 / kg]]> 4339.03

[0056] Example 3

[0057] according to Figure 1 Anhydrous dysprosium fluoride is prepared in one step from metallic dysprosium reduction slag.

[0058] The composition of the dysprosium metal reduction slag is shown in Table 5.

[0059] Table 5 Composition of metal dysprosium reduction slag

[0060] Element RE F Ca Mass percentage (%) 5.97 46.80 47.23

[0061] Take 1.0kg of metallic dysprosium reduction slag and crush it with a jaw crusher. After crushing, place it in a ball mill for ball milling. Pour the ball-milled material into a 10L plastic measuring cup and mix it with 6L of pure water. After mixing, obtain the supernatant and water-leached slag. Slowly add 1.5mol / L hydrochloric acid dropwise into the water-leached slag slurry. When the slurry is adjusted to a pH value of 1.0, stop adding hydrochloric acid, perform solid-liquid separation, and set the stirring speed to 120r / min. The separated solid (calculated as fluorine in the metallic dysprosium reduction slag) is mixed with 1.3 mol / L dysprosium chloride liquid (REO) in a molar ratio of 3:1.8. The mixed slurry is placed in a 20L high-pressure reactor, covered with a sealing cover, and stirred. A precipitation conversion reaction is carried out under high temperature conditions. The acid value of the liquid is adjusted to pH 1 using analytically pure ammonium bicarbonate. The reaction time is controlled to be 260 min, the stirring speed is 230 r / min, the reaction temperature is controlled to be 200°C, and filtration is used for solid-liquid separation. The separated fluoride is washed with pure water at a mass ratio of 1:62. The washed fluoride is dried at 102°C for 360 min. After drying, vacuum is evacuated until the vacuum degree reaches minus 40 kPa. Vacuuming is stopped and heating is continued. When the temperature reaches 800°C, it is kept warm for 120 min. The central particle size of the generated fluoride is 1.08 um, O is 0.050%, Ca is 0.41%, and the fluorine conversion rate reaches 98.5%. Excess dysprosium chloride and calcium chloride mixed solution is extracted by fractionation of organic phase with P507: kerosene-2:1 to separate metallic dysprosium from calcium chloride, and the separated terbium liquid is used as raw material to ensure that the rare earth liquid and rare earth reduction slag can be recovered. The acidified water of the reduction slag and the organic phase washing water are neutralized with the soaking liquid of the reduction slag and pure water, and there is no wastewater discharge in the whole process.

[0062] Table 6 Particle size distribution data of anhydrous dysprosium fluoride crystals prepared in Example 3

[0063] project result <![CDATA[D 10 / μm]]> 0.51 <![CDATA[D 25 / μm]]> 0.71 <![CDATA[D 50 / μm]]> 1.08 <![CDATA[D 75 / μm]]> 1.78 <![CDATA[D 90 / μm]]> 2.73 <![CDATA[D 97 / μm]]> 3.90 <![CDATA[D 100 / μm]]> 5.66 <![CDATA[D (3,2) / μm]]> 0.94 <![CDATA[D (4,3) / μm]]> 1.39 Span 2.06 <![CDATA[Specific surface area by weight / m 2 / kg]]> 6363.08

[0064] Example 4

[0065] according to Figure 1 Anhydrous yttrium fluoride is prepared in one step by using metallic yttrium reduction slag.

[0066] The composition of the metal yttrium reduction slag is shown in Table 7.

[0067] Table 7 Composition of metal yttrium reduction slag

[0068] Element RE F Ca Mass percentage (%) 0.75 45.6 53.65

[0069] Take 1.0kg of metallic yttrium reduction slag and crush it with a jaw crusher. After crushing, place it in a ball mill for ball milling. Pour the ball-milled material into a 10L plastic measuring cup and mix it with 8L of pure water. After mixing, obtain the supernatant and water-leached slag. Slowly add 2mol / L hydrochloric acid dropwise into the water-leached slag slurry. When the slurry is adjusted to a pH value of 1.0, stop adding hydrochloric acid, perform solid-liquid separation, and set the stirring speed to 120r / min. The separated solid (calculated as fluorine in the metal yttrium reduction slag) is mixed with 1.25 mol / L dysprosium chloride liquid (REO) in a molar ratio of 3:2.0, and the mixed slurry is placed in a 20L high-pressure reactor, covered with a sealing cover, and stirred, and a precipitation conversion reaction is carried out under high temperature conditions. The acid value of the liquid is adjusted to a pH of 2 using analytically pure ammonium bicarbonate, the reaction time is controlled to 270 min, the stirring speed is 260 r / min, the reaction temperature is controlled to 190°C, and filtration is used for solid-liquid separation. The separated fluoride is washed with pure water, and the washing mass ratio is 1:59. The washed fluoride is dried at 105°C for 300 min. After drying, vacuum is evacuated until the vacuum degree reaches minus 20 kPa, and vacuum is stopped. Heating is continued. When the temperature reaches 700°C, it is kept warm for 240 min. The central particle size of the generated fluoride is 1.60 um, O is 0.039%, Ca is 0.58%, and the fluorine conversion rate reaches 98.59%. Excess yttrium chloride and calcium chloride mixed solution is extracted by fractionation of organic phase with P507: kerosene-2:1 to separate metallic yttrium from calcium chloride. The separated terbium liquid is used as raw material to ensure that the rare earth liquid and rare earth reduction slag can be recovered. The acidified water of the reduction slag and the organic phase washing water are neutralized with the soaking liquid of the reduction slag and pure water, and there is no wastewater discharge in the whole process.

[0070] Table 8 Particle size distribution data of anhydrous yttrium fluoride crystals prepared in Example 4

[0071] project result <![CDATA[D 10 / μm]]> 0.74 <![CDATA[D 25 / μm]]> 1.03 <![CDATA[D 50 / μm]]> 1.60 <![CDATA[D 75 / μm]]> 2.54 <![CDATA[D 90 / μm]]> 3.50 <![CDATA[D 97 / μm]]> 4.72 <![CDATA[D 100 / μm]]> 7.17 <![CDATA[D (3,2) / μm]]> 1.36 <![CDATA[D (4,3) / μm]]> 1.91 Span 1.73 <![CDATA[Specific surface area by weight / m 2 / kg]]> 4427.63

[0072] Example 5

[0073] according to Figure 1 Anhydrous gadolinium fluoride is prepared in one step from metallic gadolinium reduction slag.

[0074] The composition of the metallic gadolinium reduced slag is shown in Table 9.

[0075] Table 9 Composition of metal gadolinium reduction slag

[0076] Element RE F Ca Mass percentage (%) 0.68 43.81 55.51

[0077] 1.0 kg of metallic gadolinium reduction slag was crushed with a jaw crusher, and then placed in a ball mill for ball milling. The ball-milled material was poured into a 10 L plastic measuring cup and mixed with 5 L of pure water to obtain a supernatant and water-leached slag. 2 mol / L hydrochloric acid was slowly added dropwise to the water-leached slag slurry. When the slurry was adjusted to a pH value of 1.2, the addition of hydrochloric acid was stopped for solid-liquid separation, and the stirring speed was set to 160 r / min. The separated solid (calculated as fluorine in the metallic gadolinium reduction slag) is mixed with 1.4 mol / L dysprosium chloride liquid (REO) in a molar ratio of 3:2.6. The mixed slurry is placed in a 20L high-pressure reactor, covered with a sealing cover, and stirred. A precipitation conversion reaction is carried out under high temperature conditions. The acid value of the liquid is adjusted to a pH of 3.5 using analytically pure ammonium bicarbonate. The reaction time is controlled to 300 min, the stirring speed is 220 r / min, the temperature is controlled to 200° C., and a filtration method is used for solid-liquid separation. The separated fluoride is washed with pure water at a washing mass ratio of 1:60. The washed fluoride is dried at 105° C. for 360 min. After drying, vacuum is evacuated until the vacuum degree reaches 30 kPa. The vacuum is stopped, and heating is continued. When the temperature reaches 760° C., the temperature is kept for 300 min. The central particle size of the generated fluoride is 5.12 um, O is 0.042%, Ca is 0.25%, and the fluorine conversion rate reaches 99.10%. Excessive mixed solution of gadolinium chloride and calcium chloride is extracted by fractionation of organic phase of P507: kerosene-2:1 to separate metallic gadolinium from calcium chloride, and the separated terbium liquid is used as raw material to ensure that the rare earth liquid and rare earth reduction slag can be recovered. The acidified water of the reduction slag and the organic phase washing water are neutralized with the soaking liquid of the reduction slag and pure water, and there is no wastewater discharge in the whole process.

[0078] Table 10 Particle size distribution data of anhydrous gadolinium fluoride crystals prepared in Example 5

[0079]

[0080]

Claims

1. A one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag, characterized in that: include: Step 1: The blocky rare earth reduction slag is crushed and ball-milled into powder; Step 2: Mix the powder obtained in step 1 with pure water, remove the generated gas under stirring, and obtain a supernatant and water-leached residue after standing. The water-leached residue is further subjected to acidification, filtration, and water washing to obtain treated rare earth reduction residue; Step 3: The treated rare earth reduction slag obtained in step 2 is mixed with the same type of rare earth chloride feed liquid, the mixed slurry is placed in a high-pressure reactor, a sealing cover is put on, stirring is started, a precipitation conversion reaction is carried out under high temperature conditions, and rare earth fluoride and filtrate are obtained by filtering; Step 4: The rare earth fluoride obtained in step 3 is subjected to washing, drying, vacuuming and roasting processes to obtain anhydrous rare earth fluoride; Step 5: The filtrate obtained in step 3 contains rare earth chloride and calcium chloride. The rare earth is enriched using P507 extractant and returned to step 3 for recycling.

2. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: The rare earth reduction slag in step 1 includes one or more of metal terbium reduction slag, metal dysprosium reduction slag, metal yttrium reduction slag, and metal gadolinium reduction slag.

3. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: The components of the rare earth reduction slag in step 1 include Ca: 45-57%, F: 40-49%, and RE: 0.6-10%.

4. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In step 2, the mass ratio of rare earth reduction slag powder to pure water is 1:3-10, and the stirring speed is 100-160 r / min.

5. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In step 2, 0.5-3 mol / L hydrochloric acid is used for acidification, and the pH of the solution after acidification is 0.5-1.

5. After filtering, it is washed with pure water, and the acid water obtained by filtering is neutralized with the supernatant.

6. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In step three, the concentration of the rare earth chloride solution is 1.0 mol / L to 1.5 mol / L, the pH of the rare earth solution is adjusted to 1 to 4 by using ammonium bicarbonate, the input amount of the rare earth reduction slag and the input amount of the rare earth solution are calculated according to the molar ratio of fluorine in the rare earth reduction slag to REO in the rare earth solution, and the molar ratio of fluorine in the rare earth reduction slag to REO in the rare earth solution is 3:1.0 to 3.

0.

7. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In the step 3, the precipitation conversion reaction temperature is 90-200° C., the stirring speed is 150-300 r / min, and the reaction time is 200-300 min.

8. The one-step process for preparing anhydrous rare earth fluoride from rare earth reduction slag according to claim 1, characterized in that: In the step 4, pure water is used for washing, and the mass ratio of rare earth fluoride to pure water is 1:50-70. The washed rare earth fluoride is dried at a temperature of 100-110°C for 180-480 minutes. After drying, vacuum is drawn to a vacuum degree of -50 kPa to -20 kPa, and the vacuum is turned off for roasting at a temperature of 600-800°C for 120-360 minutes.

Citation Information

Patent Citations

  • Recovery method of rare earth metal electrolysis fused salt slag

    CN105567985A

  • Method for efficiently removing fluorine from fluorine-containing mixed rare earth chloride solution

    CN114182113A

  • Method for extracting rare earth and recovering fluorine from bastnaesite optimal leaching residues