Preparation process of wear-resistant aluminum alloy material for smart watch

By spraying modified nanoalumina on the surface of the aluminum alloy and impregnating functional polysiloxane, the corrosion problem of aluminum alloy in high Cl-concentration environment is solved, and its wear resistance and corrosion resistance is improved, and the silver ions are used to achieve the corrosion resistance of aluminum alloy. The photothermal effect achieves self-healing and extends service life.

CN119040686AInactive Publication Date: 2024-11-29HAIAN HONGYU ALLOY MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411557335.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Aluminum alloys are prone to pitting in high Cl-concentration corrosion environments, which affects its service life and field. They are prone to rust when exposed to sweat in human body and require corrosion protection.

Method used

Using a combination of modified nanoalumina and functional polysiloxane, the wear-resistant aluminum alloy material for smart watches is formed by spraying modified nanoalumina and impregnating it with functional polysiloxane, which enhances the wear-resistant aluminum alloy material for smart watches. Its corrosion resistance and wear resistance.

Benefits of technology

It significantly improves the corrosion resistance and antibacterial effect of aluminum alloys, and realizes self-healing through the photothermal effect of silver ions, extends the service life and expands the application field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention discloses a preparation process of a wear-resistant aluminum alloy material for a smart watch, and relates to the field of aluminum alloys. When the wear-resistant aluminum alloy material for the smart watch is prepared, an aluminum-silicon alloy and a copper-phosphorus alloy are mixed and then mixed with an aluminum-silicon-magnesium alloy and metal neodymium, and a precursor aluminum alloy is obtained; the preparation method comprises the following steps: reacting tetramethyl tetravinyl cyclotetrasiloxane with chloromethyl pentamethyldisiloxane, and then reacting with N, N-dimethyl-3-(trimethoxysilyl)-1-propylamine to obtain functional polysiloxane; the preparation method comprises the following steps: preparing aluminum isopropoxide into gel balls, loading silver ions on the gel balls, and sequentially reacting the gel balls with hydroxymethyl triethoxysilane and 4-carboxyl-2, 2, 6, 6-tetramethyl azacyclohexane-1-oxyl free radicals to obtain modified nano aluminum oxide; and the modified nanometer aluminum oxide is sprayed on the precursor aluminum alloy, then the precursor aluminum alloy is impregnated with functional polysiloxane, and the wear-resistant aluminum alloy material for the intelligent watch is prepared. The wear-resistant aluminum alloy material for the intelligent watch prepared through the method has excellent wear resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of aluminum alloys, and in particular to a preparation process of a wear-resistant aluminum alloy material for a smart watch. Background Art

[0002] With the rapid development of aerospace, high-speed rail, shipbuilding, communications and other industries, the related research on high-strength and high-conductivity aluminum alloy materials has attracted great attention. Aluminum alloys are considered to be an important guarantee for lightweight and sustainable development due to their unique properties. Aluminum alloys are obtained by adding some other metals or non-metallic elements to pure non-ferrous aluminum and melting them. Not only does it have the characteristics of pure aluminum, but also due to the alloying effect, the comprehensive properties of aluminum alloys are greatly improved, so that aluminum alloys have higher specific strength, hardness, wear resistance and other excellent comprehensive properties, and their application range is becoming wider and wider. However, due to the high activity of aluminum, in high Cl - Corrosion phenomena such as pitting are prone to occur in corrosive environments such as high concentrations. The sweat secreted by the human body contains sodium chloride, which can easily cause rust on metal materials when bare hands touch metal products. In order to extend the service life of aluminum alloys, expand the use of aluminum alloys, and save resources, it is necessary to perform corrosion protection treatment on aluminum alloys. Therefore, the present invention prepares an aluminum alloy material for smart watches with excellent corrosion resistance. Summary of the invention

[0003] The purpose of the present invention is to provide a preparation process of wear-resistant aluminum alloy material for smart watches to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: A wear-resistant aluminum alloy material for a smart watch is obtained by spraying modified nano-aluminum oxide on the surface of a precursor aluminum alloy and then impregnating it with functional polysiloxane.

[0005] As an optimization, the precursor aluminum alloy is obtained by mixing aluminum silicon alloy and copper phosphorus alloy, and then mixing with aluminum silicon magnesium alloy and metal neodymium.

[0006] As an optimization, the aluminum-silicon alloy model is Al-Si20, which comes from Suzhou Haichuan Rare Metal Products Co., Ltd.

[0007] As an optimization, the copper-phosphorus alloy model is Cu-P14, which comes from Suzhou Haichuan Rare Metal Products Co., Ltd.

[0008] As an optimization, the aluminum-silicon-magnesium alloy model is AlSi10Mg, which comes from Hunan 369 Metallurgical Technology Co., Ltd.

[0009] As an optimization, the metal neodymium comes from Ganzhou Xiyou New Materials Co., Ltd.

[0010] As an optimization, the modified nano-alumina is prepared by making gel balls from aluminum isopropoxide, loading silver ions, and then reacting with hydroxymethyltriethoxysilane and 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radicals in sequence.

[0011] As an optimization, the functional polysiloxane is obtained by reacting tetramethyltetravinylcyclotetrasiloxane with chloromethylpentamethyldisiloxane and then reacting with N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine.

[0012] A preparation process of a wear-resistant aluminum alloy material for a smart watch, comprising the following preparation steps: (1) Melt the aluminum silicon alloy in a crucible resistance furnace, keep it at 750-850℃ for 5-15min in an argon atmosphere, add copper-phosphorus alloy (0.9-1.1 times the mass of the aluminum silicon alloy), stir and melt it in a quartz tube preheated to 150-250℃ at a speed of 250-350r / min, keep it warm for 15-25min, heat it to 1600-1800℃ and keep it warm for 4-6min, cool it to 190-210℃ with the furnace, take it out and break it into small pieces, put it into an alumina ball mill, add anhydrous ethanol (1-2 times the mass of the mixed powder), ball mill it at 250-350r / min for 7-9h, sieve it through 150-250 mesh, and dry it at 80-90℃ for 10-12h to obtain an intermediate alloy; (2) The aluminum-silicon-magnesium alloy is melted at 700-800°C in a silicon carbide furnace, and a refining agent of 0.004-0.006 times the mass of the aluminum-silicon alloy is added, and the alloy is kept at 800-900°C for 5-15 minutes, and the surface oxidation scum is scraped off, and metal neodymium of 0.005-0.015 times the mass of the aluminum-silicon alloy and an intermediate alloy of 0.01-0.03 times the mass of the aluminum-silicon alloy are added, and the alloy is kept at this temperature for 10-20 minutes. Ultrasonic treatment at 15-25kHz for 10-20 minutes is performed, and the alloy is poured into a metal mold preheated to 190-210°C, and the alloy is cooled and formed to obtain a precursor aluminum alloy; (3) Tetramethyltetravinylcyclotetrasiloxane, chloromethylpentamethyldisiloxane and tetramethylammonium hydroxide siliconate are mixed in a mass ratio of 1:(0.3-0.4):(0.01-0.03), nitrogen is passed through for 5-15 min, stirred at 95-105°C and 100-200 rpm for 7-9 h, then heated to 130-140°C at a rate of 10-20°C / min and stirred for 40-50 min, and distilled at 0.1-0.3 MPa for 1-2 h to obtain a polysiloxane precursor; the polysiloxane precursor and anhydrous ethanol are mixed in a mass ratio of 1:( 24-26), stir at 85-95° C. and 200-300 rpm for 20-30 min in a nitrogen atmosphere, add N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine, wherein the molar amount of chlorine atoms in the polysiloxane precursor and the molar amount of tertiary amine groups in N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine are 1:1, continue stirring for 29-31 h, rotary evaporate at 50-60° C. for 1-2 h, extract with petroleum ether for 3-5 times, and dry at 85-95° C. for 23-25 ​​h to obtain functional polysiloxane; (4) The porous silver-loaded nanoalumina and anhydrous ethanol were mixed in a mass ratio of 1:(20-30), stirred at 20-30°C and 100-200 rpm for 1-3 h, 0.3-0.5 times the mass of the porous silver-loaded nanoalumina hydroxymethyltriethoxysilane was added, the temperature was raised to 70-80°C and stirring was continued for 3-5 h, the mixture was naturally cooled to room temperature and filtered, dried at 115-125°C for 8-10 h, and calcined at 1000-1200°C for 1 h. ~3h to obtain pre-modified nano-alumina; the pre-modified nano-alumina, 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radical and acetonitrile are mixed in a mass ratio of 1:(1.2~1.4):(20~30), stirred at 20~30°C and 200~300rpm for 23~25h, filtered, washed with anhydrous ethanol for 3~5 times, and dried at 70~80°C for 10~12h to obtain modified nano-alumina; (5) The modified nano-alumina was sprayed on the precursor aluminum alloy preheated to 140-160°C to a thickness of 90-100 μm under the conditions of sandblasting pressure of 0.4-0.6 MPa, spraying distance of 115-125 mm, and powder feeding rate of 15-25 g / min, and then dried at 115-125°C for 1-3 h. The modified nano-alumina was then ultrasonically immersed in a functional polysiloxane solution for 4-6 min, taken out, allowed to stand at 20-30°C for 25-35 min, and dried at 145-155°C for 8-10 h to obtain a wear-resistant aluminum alloy material for smart watches.

[0013] As an optimization, the refining agent in step (2) is obtained by mixing potassium chloride, sodium chloride and sodium hexafluoroaluminate in a mass ratio of 1:0.64:0.49.

[0014] As an optimization, the reaction equation of the polysiloxane precursor in step (3) is: .

[0015] As an optimization, the reaction equation of the functional polysiloxane in step (3) is: .

[0016] As an optimization, the porous silver-loaded nano-alumina in step (4) is prepared by mixing aluminum isopropoxide and deionized water in a mass ratio of 1:2, stirring at 85°C and 150 rpm for 60 min, adding a 1 mol / L nitric acid solution of 0.4 times the mass of aluminum isopropoxide, heating to 100°C for aging for 7 h, distilling at 85°C for 1 h, dropping the ball into an oil-ammonia column with a dropper, and pouring out to obtain a gel ball; washing the gel ball with isopropanol 4 times, standing at 25°C for 24 h, and then drying at 110°C for 8 h, moving it into a muffle furnace, heating to 600°C at 3°C / min and calcining it for 4 h, taking it out and naturally cooling it to room temperature, immersing it in a 25 g / L silver nitrate solution for 2 h, filtering it, washing it with anhydrous ethanol 4 times, drying it at 75°C for 11 h, and calcining it at 300°C for 2 h.

[0017] As an optimization, the reaction equation of the pre-modified nano-alumina in step (4) is: .

[0018] As an optimization, the reaction equation for modifying the nano-alumina in step (4) is: .

[0019] As an optimization, the functional polysiloxane solution in step (5) is obtained by mixing the functional polysiloxane and an ethanol solution with a volume fraction of 75% in a mass ratio of 1:5.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are: When preparing the wear-resistant aluminum alloy material for smart watches, the present invention comprises the following steps: mixing aluminum silicon alloy and copper phosphorus alloy to obtain an intermediate alloy; mixing aluminum silicon magnesium alloy, metal neodymium and the intermediate alloy to obtain a precursor aluminum alloy; reacting tetramethyltetravinylcyclotetrasiloxane with chloromethylpentamethyldisiloxane, and then reacting with N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine to obtain functional polysiloxane; preparing aluminum isopropoxide into gel balls, loading silver ions, and then reacting with hydroxymethyltriethoxysilane and 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radicals in sequence to obtain modified nano aluminum oxide; spraying the modified nano aluminum oxide on the precursor aluminum alloy, and then immersing the modified nano aluminum oxide in a functional polysiloxane solution to prepare the wear-resistant aluminum alloy material for smart watches.

[0021] First, aluminum silicon alloy and copper phosphorus alloy are mixed to obtain an intermediate alloy; aluminum silicon magnesium alloy, metal neodymium and the intermediate alloy are mixed to obtain a precursor aluminum alloy; tetramethyltetravinylcyclotetrasiloxane and chloromethylpentamethyldisiloxane are reacted, and then reacted with N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine to obtain a functional polysiloxane; the intermediate alloy is prepared by adding phosphorus element and rare earth element neodymium to form aluminum phosphide to provide a nucleation base for primary silicon crystals, and at the same time, rare earth elements are enriched at the tips of eutectic silicon dendrites, synergistically promoting grain refinement, and improving the casting performance and corrosion resistance of wear-resistant aluminum alloy materials for smart watches; a functional polysiloxane with a quaternary ammonium structure is synthesized by a quaternary ammonium reaction, and chloride ions in sweat are adsorbed by electrostatic action, thereby improving the corrosion resistance of wear-resistant aluminum alloy materials for smart watches.

[0022] Secondly, aluminum isopropoxide is made into gel balls and then loaded with silver ions, which are then reacted with hydroxymethyltriethoxysilane and 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radicals in sequence to obtain modified nano-alumina; the modified nano-alumina is sprayed on the precursor aluminum alloy and then immersed in a functional polysiloxane solution to prepare a wear-resistant aluminum alloy material for smart watches; loading silver ions in porous alumina can reduce the reaction between sweat and bacteria and improve the antibacterial effect of the wear-resistant aluminum alloy material for smart watches; at the same time, the photothermal effect generated by silver ions under near-infrared light irradiation can promote the cross-linking self-repair of alkoxyamines and carbon-carbon double bonds, repair minor damage and defects on the alloy surface, and improve the wear resistance of the wear-resistant aluminum alloy material for smart watches; after spraying an alumina ceramic coating on the precursor aluminum alloy, the pores are sealed by impregnation with functional polysiloxane to further enhance the wear resistance of the wear-resistant aluminum alloy material for smart watches. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example

[0024] A preparation process of a wear-resistant aluminum alloy material for a smart watch, the preparation process of the wear-resistant aluminum alloy material for a smart watch comprising the following preparation steps: (1) Melt the aluminum silicon alloy in a crucible resistance furnace, keep it at 750℃ for 15min in an argon atmosphere, add copper phosphorus alloy (0.9 times the mass of the aluminum silicon alloy), stir and melt it in a quartz tube preheated to 150℃ at a speed of 250r / min, keep it warm for 25min, heat it to 1600℃ and keep it warm for 6min, cool it to 190℃ with the furnace, take it out and break it into small pieces, put it into an alumina ball mill, add anhydrous ethanol (1 times the mass of the mixed powder), ball mill it at 250r / min for 9h, sieve it through 150 mesh, and dry it at 80℃ for 12h to obtain an intermediate alloy; (2) The aluminum-silicon-magnesium alloy was melted at 700°C in a silicon carbide furnace, and a refining agent of 0.004 times the mass of the aluminum-silicon alloy was added. The alloy was kept at 800°C for 15 minutes, and the surface oxidation scum was scraped off. Metal neodymium of 0.005 times the mass of the aluminum-silicon alloy and an intermediate alloy of 0.01 times the mass of the aluminum-silicon alloy were added. The alloy was kept at this temperature for 20 minutes, and ultrasonic treatment was performed at 15kHz for 20 minutes. The alloy was poured into a metal mold preheated to 190°C, and the alloy was cooled and formed to obtain a precursor aluminum alloy. (3) Tetramethyltetravinylcyclotetrasiloxane, chloromethylpentamethyldisiloxane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:0.3:0.01, nitrogen was passed through for 5 minutes, stirred at 95°C and 100 rpm for 9 hours, then heated to 140°C at a rate of 10°C / min and continued to stir for 40 minutes, and distilled at 0.1 MPa for 2 hours to obtain a polysiloxane precursor; the polysiloxane precursor and anhydrous ethanol were mixed in a mass ratio of 1:24, and In a nitrogen atmosphere, the mixture was stirred at 85° C. and 200 rpm for 30 min, and N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine was added, wherein the ratio of the molar amount of chlorine atoms in the polysiloxane precursor to the molar amount of tertiary amine groups in N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine was 1:1, and the stirring was continued for 31 h. The mixture was rotary evaporated at 50° C. for 2 h, extracted with petroleum ether for 3 times, and dried at 85° C. for 25 h to obtain a functional polysiloxane. (4) The porous silver-loaded nano-alumina and anhydrous ethanol were mixed in a mass ratio of 1:20, stirred at 20°C and 100 rpm for 3 h, 0.3 times the mass of the porous silver-loaded nano-alumina hydroxymethyltriethoxysilane was added, the temperature was raised to 70°C and the stirring was continued for 5 h, the mixture was naturally cooled to room temperature and filtered, dried at 115°C for 10 h, and calcined at 1000°C for 3 h to obtain pre-modified nano-alumina; the pre-modified nano-alumina, 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radical and acetonitrile were mixed in a mass ratio of 1:1.2:20, stirred at 20°C and 200 rpm for 25 h, filtered, washed with anhydrous ethanol 5 times, and dried at 70°C for 12 h to obtain modified nano-alumina; (5) The modified nano-alumina was sprayed on the precursor aluminum alloy preheated to 140°C to a thickness of 90 μm under the conditions of sandblasting pressure of 0.4 MPa, spraying distance of 115 mm, and powder feeding rate of 15 g / min, dried at 115°C for 3 h, ultrasonically immersed in a functional polysiloxane solution for 4 min, taken out, allowed to stand at 20°C for 35 min, and dried at 145°C for 10 h to obtain a wear-resistant aluminum alloy material for smart watches. Example

[0025] A preparation process of a wear-resistant aluminum alloy material for a smart watch, the preparation process of the wear-resistant aluminum alloy material for a smart watch comprising the following preparation steps: (1) Melt the aluminum silicon alloy in a crucible resistance furnace, keep it at 800℃ for 10 minutes in an argon atmosphere, add copper phosphorus alloy with a mass equal to that of the aluminum silicon alloy, stir and melt it in a quartz tube preheated to 200℃ at a speed of 300r / min, keep it at that temperature for 20 minutes, heat it to 1700℃ and keep it at that temperature for 5 minutes, cool it to 200℃ with the furnace, take it out and break it into small pieces, put it into an alumina ball mill, add anhydrous ethanol with a mass equal to that of the mixed powder, ball mill it at 300r / min for 8 hours, sieve it through 200 mesh, and dry it at 85℃ for 11 hours to obtain an intermediate alloy; (2) The aluminum-silicon-magnesium alloy was melted at 750°C in a silicon carbide furnace, and a refining agent of 0.005 times the mass of the aluminum-silicon alloy was added. The alloy was kept at 850°C for 10 minutes, and the surface oxide scum was scraped off. Metal neodymium of 0.01 times the mass of the aluminum-silicon alloy and an intermediate alloy of 0.02 times the mass of the aluminum-silicon alloy were added. The alloy was kept at this temperature for 15 minutes, and ultrasonic treatment was performed at 20kHz for 15 minutes. The alloy was poured into a metal mold preheated to 200°C, and the alloy was cooled and formed to obtain a precursor aluminum alloy. (3) Tetramethyltetravinylcyclotetrasiloxane, chloromethylpentamethyldisiloxane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:0.35:0.02, nitrogen was passed for 10 minutes, stirred at 100°C and 150 rpm for 8 hours, then heated to 135°C at a rate of 15°C / min and continued to stir for 45 minutes, and distilled at 0.2 MPa for 1.5 hours to obtain a polysiloxane precursor; the polysiloxane precursor and anhydrous ethanol were mixed in a mass ratio of 1:25, In a nitrogen atmosphere, the mixture was stirred at 90° C. and 250 rpm for 25 min, and N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine was added, wherein the molar amount of chlorine atoms in the polysiloxane precursor and the molar amount of tertiary amine groups in N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine were in a ratio of 1:1, and the stirring was continued for 30 h. The mixture was rotary evaporated at 55° C. for 1.5 h, extracted with petroleum ether for 4 times, and dried at 90° C. for 24 h to obtain a functional polysiloxane. (4) The porous silver-loaded nano-alumina and anhydrous ethanol were mixed in a mass ratio of 1:25, stirred at 25°C and 150 rpm for 2 hours, 0.4 times the mass of the porous silver-loaded nano-alumina hydroxymethyltriethoxysilane was added, the temperature was raised to 75°C and the stirring was continued for 4 hours, the mixture was naturally cooled to room temperature and filtered, dried at 120°C for 9 hours, and calcined at 1100°C for 2 hours to obtain pre-modified nano-alumina; the pre-modified nano-alumina, 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radical and acetonitrile were mixed in a mass ratio of 1:1.3:25, stirred at 25°C and 250 rpm for 24 hours, filtered, washed with anhydrous ethanol 4 times, and dried at 75°C for 11 hours to obtain modified nano-alumina; (5) The modified nano-alumina was sprayed on the precursor aluminum alloy preheated to 150°C to a thickness of 95 μm under the conditions of sandblasting pressure of 0.5 MPa, spraying distance of 120 mm, and powder feeding rate of 20 g / min, dried at 120°C for 2 h, ultrasonically immersed in a functional polysiloxane solution for 5 min, taken out, allowed to stand at 25°C for 30 min, and dried at 150°C for 9 h to obtain a wear-resistant aluminum alloy material for smart watches. Example

[0026] A preparation process of a wear-resistant aluminum alloy material for a smart watch, the preparation process of the wear-resistant aluminum alloy material for a smart watch comprising the following preparation steps: (1) Melt the aluminum silicon alloy in a crucible resistance furnace, keep it at 850℃ for 5 minutes in an argon atmosphere, add copper phosphorus alloy with a mass 1.1 times that of the aluminum silicon alloy, stir and melt it in a quartz tube preheated to 250℃ at a speed of 350r / min, keep it warm for 15 minutes, heat it to 1800℃ and keep it warm for 4 minutes, cool it to 210℃ with the furnace, take it out and break it into small pieces, put it into an alumina ball mill, add anhydrous ethanol with a mass 2 times that of the mixed powder, ball mill it at 350r / min for 7 hours, sieve it through 250 mesh, and dry it at 90℃ for 10 hours to obtain an intermediate alloy; (2) The aluminum-silicon-magnesium alloy was melted at 800°C in a silicon carbide furnace, and a refining agent of 0.006 times the mass of the aluminum-silicon alloy was added. The alloy was kept at 900°C for 5 minutes, and the surface oxide scum was scraped off. Metal neodymium of 0.015 times the mass of the aluminum-silicon alloy and an intermediate alloy of 0.03 times the mass of the aluminum-silicon alloy were added. The alloy was kept at this temperature for 10 minutes, and ultrasonic treatment was performed at 25kHz for 10 minutes. The alloy was poured into a metal mold preheated to 210°C, and the alloy was cooled and formed to obtain a precursor aluminum alloy. (3) Tetramethyltetravinylcyclotetrasiloxane, chloromethylpentamethyldisiloxane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:0.4:0.03, nitrogen was passed for 15 minutes, stirred at 105°C and 200 rpm for 7 hours, then heated to 130°C at a rate of 20°C / min and continued to stir for 50 minutes, and distilled at 0.3 MPa for 1 hour to obtain a polysiloxane precursor; the polysiloxane precursor and anhydrous ethanol were mixed in a mass ratio of 1:26, In a nitrogen atmosphere, the mixture was stirred at 95° C. and 300 rpm for 20 min, and N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine was added, wherein the ratio of the molar amount of chlorine atoms in the polysiloxane precursor to the molar amount of tertiary amine groups in N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine was 1:1, and the mixture was stirred for 29 h. The mixture was rotary evaporated at 60° C. for 1 h, extracted with petroleum ether for 5 times, and dried at 95° C. for 23 h to obtain a functional polysiloxane. (4) The porous silver-loaded nano-alumina and anhydrous ethanol were mixed in a mass ratio of 1:30, stirred at 30°C and 200 rpm for 1 hour, 0.5 times the mass of the porous silver-loaded nano-alumina hydroxymethyltriethoxysilane was added, the temperature was raised to 80°C and the stirring was continued for 3 hours, the mixture was naturally cooled to room temperature and filtered, dried at 125°C for 8 hours, and calcined at 1200°C for 1 hour to obtain pre-modified nano-alumina; the pre-modified nano-alumina, 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radical and acetonitrile were mixed in a mass ratio of 1:1.4:30, stirred at 30°C and 300 rpm for 23 hours, filtered, washed with anhydrous ethanol 5 times, and dried at 80°C for 10 hours to obtain modified nano-alumina; (5) The modified nano-alumina was sprayed on the precursor aluminum alloy preheated to 160°C to a thickness of 100 μm under the conditions of sandblasting pressure of 0.6 MPa, spraying distance of 125 mm, and powder feeding rate of 25 g / min, dried at 125°C for 1 h, ultrasonically immersed in a functional polysiloxane solution for 6 min, taken out, allowed to stand at 30°C for 25 min, and dried at 155°C for 8 h to obtain a wear-resistant aluminum alloy material for smart watches.

[0027] Comparative Example 1 A preparation process of a wear-resistant aluminum alloy material for a smart watch, the preparation process of the wear-resistant aluminum alloy material for a smart watch comprising the following preparation steps: (1) The aluminum-silicon-magnesium alloy was melted at 750°C in a silicon carbide furnace, and a refining agent of 0.005 times the mass of the aluminum-silicon alloy was added. The alloy was kept at 850°C for 10 minutes, and the surface oxidation scum was scraped off. The aluminum-silicon alloy of 0.02 times the mass of the aluminum-silicon alloy was added, and the alloy was kept at this temperature for 15 minutes. The alloy was ultrasonically treated at 20kHz for 15 minutes, and then poured into a metal mold preheated to 200°C, and cooled to obtain a precursor aluminum alloy. (2) Tetramethyltetravinylcyclotetrasiloxane, chloromethylpentamethyldisiloxane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:0.35:0.02, nitrogen was passed for 10 minutes, stirred at 100°C and 150 rpm for 8 hours, then heated to 135°C at a rate of 15°C / min and continued to stir for 45 minutes, and distilled at 0.2 MPa for 1.5 hours to obtain a polysiloxane precursor; the polysiloxane precursor and anhydrous ethanol were mixed in a mass ratio of 1:25, In a nitrogen atmosphere, the mixture was stirred at 90° C. and 250 rpm for 25 min, and N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine was added, wherein the molar amount of chlorine atoms in the polysiloxane precursor and the molar amount of tertiary amine groups in N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine were in a ratio of 1:1, and the stirring was continued for 30 h. The mixture was rotary evaporated at 55° C. for 1.5 h, extracted with petroleum ether for 4 times, and dried at 90° C. for 24 h to obtain a functional polysiloxane. (3) The porous silver-loaded nano-alumina and anhydrous ethanol were mixed in a mass ratio of 1:25, stirred at 25°C and 150 rpm for 2 hours, 0.4 times the mass of the porous silver-loaded nano-alumina hydroxymethyltriethoxysilane was added, the temperature was raised to 75°C and the stirring was continued for 4 hours, the mixture was naturally cooled to room temperature and filtered, dried at 120°C for 9 hours, and calcined at 1100°C for 2 hours to obtain pre-modified nano-alumina; the pre-modified nano-alumina, 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radical and acetonitrile were mixed in a mass ratio of 1:1.3:25, stirred at 25°C and 250 rpm for 24 hours, filtered, washed with anhydrous ethanol 4 times, and dried at 75°C for 11 hours to obtain modified nano-alumina; (4) The modified nano-alumina was sprayed on the precursor aluminum alloy preheated to 150°C to a thickness of 95 μm under the conditions of sandblasting pressure of 0.5 MPa, spraying distance of 120 mm, and powder feeding rate of 20 g / min, dried at 120°C for 2 h, ultrasonically immersed in a functional polysiloxane solution for 5 min, taken out, allowed to stand at 25°C for 30 min, and dried at 150°C for 9 h to obtain a wear-resistant aluminum alloy material for smart watches.

[0028] Comparative Example 2 A preparation process of a wear-resistant aluminum alloy material for a smart watch, the preparation process of the wear-resistant aluminum alloy material for a smart watch comprising the following preparation steps: (1) Melt the aluminum silicon alloy in a crucible resistance furnace, keep it at 800℃ for 10 minutes in an argon atmosphere, add copper phosphorus alloy with a mass equal to that of the aluminum silicon alloy, stir and melt it in a quartz tube preheated to 200℃ at a speed of 300r / min, keep it at that temperature for 20 minutes, heat it to 1700℃ and keep it at that temperature for 5 minutes, cool it to 200℃ with the furnace, take it out and break it into small pieces, put it into an alumina ball mill, add anhydrous ethanol with a mass equal to that of the mixed powder, ball mill it at 300r / min for 8 hours, sieve it through 200 mesh, and dry it at 85℃ for 11 hours to obtain an intermediate alloy; (2) The aluminum-silicon-magnesium alloy was melted at 750°C in a silicon carbide furnace, and a refining agent of 0.005 times the mass of the aluminum-silicon alloy was added. The alloy was kept at 850°C for 10 minutes, and the surface oxide scum was scraped off. Metal neodymium of 0.01 times the mass of the aluminum-silicon alloy and an intermediate alloy of 0.02 times the mass of the aluminum-silicon alloy were added. The alloy was kept at this temperature for 15 minutes, and ultrasonic treatment was performed at 20kHz for 15 minutes. The alloy was poured into a metal mold preheated to 200°C, and the alloy was cooled and formed to obtain a precursor aluminum alloy. (3) The porous silver-loaded nano-alumina and anhydrous ethanol were mixed in a mass ratio of 1:25, stirred at 25°C and 150 rpm for 2 hours, 0.4 times the mass of the porous silver-loaded nano-alumina hydroxymethyltriethoxysilane was added, the temperature was raised to 75°C and the stirring was continued for 4 hours, the mixture was naturally cooled to room temperature and filtered, dried at 120°C for 9 hours, and calcined at 1100°C for 2 hours to obtain pre-modified nano-alumina; the pre-modified nano-alumina, 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radical and acetonitrile were mixed in a mass ratio of 1:1.3:25, stirred at 25°C and 250 rpm for 24 hours, filtered, washed with anhydrous ethanol 4 times, and dried at 75°C for 11 hours to obtain modified nano-alumina; (4) The modified nano-alumina was sprayed on the precursor aluminum alloy preheated to 150°C to a thickness of 95 μm under the conditions of sandblasting pressure of 0.5 MPa, spraying distance of 120 mm, and powder feeding rate of 20 g / min, and dried at 120°C for 2 h to obtain a wear-resistant aluminum alloy material for smart watches.

[0029] Comparative Example 3 A preparation process of a wear-resistant aluminum alloy material for a smart watch, the preparation process of the wear-resistant aluminum alloy material for a smart watch comprising the following preparation steps: (1) Melt the aluminum silicon alloy in a crucible resistance furnace, keep it at 800℃ for 10 minutes in an argon atmosphere, add copper phosphorus alloy with a mass equal to that of the aluminum silicon alloy, stir and melt it in a quartz tube preheated to 200℃ at a speed of 300r / min, keep it at that temperature for 20 minutes, heat it to 1700℃ and keep it at that temperature for 5 minutes, cool it to 200℃ with the furnace, take it out and break it into small pieces, put it into an alumina ball mill, add anhydrous ethanol with a mass equal to that of the mixed powder, ball mill it at 300r / min for 8 hours, sieve it through 200 mesh, and dry it at 85℃ for 11 hours to obtain an intermediate alloy; (2) The aluminum-silicon-magnesium alloy was melted at 750°C in a silicon carbide furnace, and a refining agent of 0.005 times the mass of the aluminum-silicon alloy was added. The alloy was kept at 850°C for 10 minutes, and the surface oxide scum was scraped off. Metal neodymium of 0.01 times the mass of the aluminum-silicon alloy and an intermediate alloy of 0.02 times the mass of the aluminum-silicon alloy were added. The alloy was kept at this temperature for 15 minutes, and ultrasonic treatment was performed at 20kHz for 15 minutes. The alloy was poured into a metal mold preheated to 200°C, and the alloy was cooled and formed to obtain a precursor aluminum alloy. (3) Tetramethyltetravinylcyclotetrasiloxane, chloromethylpentamethyldisiloxane and tetramethylammonium hydroxide siliconate were mixed in a mass ratio of 1:0.35:0.02, nitrogen was passed for 10 minutes, stirred at 100°C and 150 rpm for 8 hours, then heated to 135°C at a rate of 15°C / min and continued to stir for 45 minutes, and distilled at 0.2 MPa for 1.5 hours to obtain a polysiloxane precursor; the polysiloxane precursor and anhydrous ethanol were mixed in a mass ratio of 1:25, In a nitrogen atmosphere, the mixture was stirred at 90° C. and 250 rpm for 25 min, and N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine was added, wherein the molar amount of chlorine atoms in the polysiloxane precursor and the molar amount of tertiary amine groups in N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine were in a ratio of 1:1, and the stirring was continued for 30 h. The mixture was rotary evaporated at 55° C. for 1.5 h, extracted with petroleum ether for 4 times, and dried at 90° C. for 24 h to obtain a functional polysiloxane. (4) The precursor aluminum alloy was ultrasonically immersed in a functional polysiloxane solution for 5 minutes, then taken out, allowed to stand at 25°C for 30 minutes, and dried at 150°C for 9 hours to obtain a wear-resistant aluminum alloy material for smart watches.

[0030] Test Case 1. Wear resistance Test method: The wear-resistant aluminum alloy material for smart watches obtained in each embodiment and the control example are of the same size, and are fixed on the sample fixture under the laboratory table by Rtec-multi-function friction and wear testing machine. A Si3N4 ceramic ball with a diameter of 6 mm is used as the friction object. The friction is carried out for 30 minutes at 25°C, a frequency of 10 Hz, a load of 20 N, and a stroke of 5 mm. The specific wear rate is calculated as wear volume / load×sliding distance.

[0031] 2. Corrosion resistance Test method: Take 10mm×10mm×10mm cube samples of the wear-resistant aluminum alloy material for smart watches obtained in each embodiment and the comparative example, weigh m0, soak them in artificial sweat (urea, sodium chloride, lactic acid and deionized water are mixed in a mass ratio of 1:5:0.94:900, and sodium hydroxide is added to adjust the pH to 5.2) for 10 hours, weigh m1 again, and calculate the mass corrosion rate = m0-m1 / surface area×time*100%.

[0032] Table 1 below shows the analysis results of the wear resistance and corrosion resistance of the wear-resistant aluminum alloy materials for smart watches using Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.

[0033] Table 1 <![CDATA[Specific wear rate mm 3 / N∙m]]> <![CDATA[Corrosion rate g / m 2 ∙h]]> Example 1 <![CDATA[3.5×10 -6 ]]> 0.12 Example 2 <![CDATA[3.2×10 -6 ]]> 0.11 Example 3 <![CDATA[3.7×10 -6 ]]> 0.15 Comparative Example 1 <![CDATA[4.4×10 -6 ]]> 1.24 Comparative Example 2 <![CDATA[0.9×10 -5 ]]> 1.81 Comparative Example 3 <![CDATA[1.1×10 -5 ]]> 0.58 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the wear-resistant aluminum alloy material for smart watches prepared by the present invention has good wear resistance and corrosion resistance.

[0034] By comparison, the corrosion rates of Examples 1, 2 and 3 are slower than those of Comparative Example 1, indicating that the intermediate alloy is prepared by doping with phosphorus and rare earth element neodymium to form aluminum phosphide that provides a nucleation substrate for primary silicon. Meanwhile, the rare earth elements are enriched at the tips of eutectic silicon dendrites, synergistically promoting grain refinement and improving the corrosion resistance of wear-resistant aluminum alloy materials for smart watches.

[0035] By comparison, Examples 1, 2, and 3 have lower specific wear rates and slower corrosion rates than those of Comparative Example 2, which illustrates that the functional polysiloxane with a quaternary ammonium structure is synthesized by quaternary ammonium reaction, and chloride ions in sweat are adsorbed by electrostatic action to improve the corrosion resistance of the wear-resistant aluminum alloy material for smart watches; the functional polysiloxane is used to impregnate and seal the pores on the precursor aluminum alloy to enhance the wear resistance of the wear-resistant aluminum alloy material for smart watches.

[0036] By comparison, the specific wear rates of Examples 1, 2, and 3 are lower than those of Comparative Example 3, which indicates that spraying an alumina ceramic coating on the precursor aluminum alloy can improve the wear resistance of the wear-resistant aluminum alloy material for smart watches; at the same time, the photothermal effect of silver ions under near-infrared light irradiation can promote the cross-linking self-repair of alkoxyamines and carbon-carbon double bonds, repair minor damage and defects on the alloy surface, and further improve the wear resistance of the wear-resistant aluminum alloy material for smart watches.

[0037] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A preparation process of wear-resistant aluminum alloy material for smart watches, characterized in that: The wear-resistant aluminum alloy material for smart watches is obtained by spraying modified nano-aluminum oxide on the surface of a precursor aluminum alloy and then impregnating it with functional polysiloxane; The precursor aluminum alloy is obtained by mixing aluminum silicon alloy and copper phosphorus alloy, and then mixing with aluminum silicon magnesium alloy and metal neodymium; The modified nano-alumina is prepared by making a gel ball from aluminum isopropoxide, loading silver ions, and then reacting with hydroxymethyltriethoxysilane and 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radicals in sequence; The functional polysiloxane is obtained by reacting tetramethyltetravinylcyclotetrasiloxane with chloromethylpentamethyldisiloxane and then reacting with N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine.

2. A preparation process of wear-resistant aluminum alloy material for smart watches, characterized in that: The method comprises the following preparation steps: (1) Melt the aluminum silicon alloy in a crucible resistance furnace, keep it at 750-850℃ for 5-15min in an argon atmosphere, add copper-phosphorus alloy (0.9-1.1 times the mass of the aluminum silicon alloy), stir and melt it in a quartz tube preheated to 150-250℃ at a speed of 250-350r / min, keep it warm for 15-25min, heat it to 1600-1800℃ and keep it warm for 4-6min, cool it to 190-210℃ with the furnace, take it out and break it into small pieces, put it into an alumina ball mill, add anhydrous ethanol (1-2 times the mass of the mixed powder), ball mill it at 250-350r / min for 7-9h, sieve it through 150-250 mesh, and dry it at 80-90℃ for 10-12h to obtain an intermediate alloy; (2) The aluminum-silicon-magnesium alloy is melted at 700-800°C in a silicon carbide furnace, and a refining agent of 0.004-0.006 times the mass of the aluminum-silicon alloy is added, and the alloy is kept at 800-900°C for 5-15 minutes, and the surface oxidation scum is scraped off, and metal neodymium of 0.005-0.015 times the mass of the aluminum-silicon alloy and an intermediate alloy of 0.01-0.03 times the mass of the aluminum-silicon alloy are added, and the alloy is kept at this temperature for 10-20 minutes. Ultrasonic treatment at 15-25kHz for 10-20 minutes is performed, and the alloy is poured into a metal mold preheated to 190-210°C, and the alloy is cooled and formed to obtain a precursor aluminum alloy; (3) Tetramethyltetravinylcyclotetrasiloxane, chloromethylpentamethyldisiloxane and tetramethylammonium hydroxide siliconate are mixed in a mass ratio of 1:(0.3-0.4):(0.01-0.03), nitrogen is passed through for 5-15 min, stirred at 95-105°C and 100-200 rpm for 7-9 h, then heated to 130-140°C at a rate of 10-20°C / min and stirred for 40-50 min, and distilled at 0.1-0.3 MPa for 1-2 h to obtain a polysiloxane precursor; the polysiloxane precursor and anhydrous ethanol are mixed in a mass ratio of 1:( 24-26), stir at 85-95° C. and 200-300 rpm for 20-30 min in a nitrogen atmosphere, add N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine, wherein the molar amount of chlorine atoms in the polysiloxane precursor and the molar amount of tertiary amine groups in N,N-dimethyl-3-(trimethoxysilyl)-1-propylamine are 1:1, continue stirring for 29-31 h, rotary evaporate at 50-60° C. for 1-2 h, extract with petroleum ether for 3-5 times, and dry at 85-95° C. for 23-25 ​​h to obtain functional polysiloxane; (4) The porous silver-loaded nanoalumina and anhydrous ethanol were mixed in a mass ratio of 1:(20-30), stirred at 20-30°C and 100-200 rpm for 1-3 h, 0.3-0.5 times the mass of the porous silver-loaded nanoalumina hydroxymethyltriethoxysilane was added, the temperature was raised to 70-80°C and stirring was continued for 3-5 h, the mixture was naturally cooled to room temperature and filtered, dried at 115-125°C for 8-10 h, and calcined at 1000-1200°C for 1 h. ~3h to obtain pre-modified nano-alumina; the pre-modified nano-alumina, 4-carboxyl-2,2,6,6-tetramethylazacyclohexane-1-oxyl free radical and acetonitrile are mixed in a mass ratio of 1:(1.2~1.4):(20~30), stirred at 20~30°C and 200~300rpm for 23~25h, filtered, washed with anhydrous ethanol for 3~5 times, and dried at 70~80°C for 10~12h to obtain modified nano-alumina; (5) The modified nano-alumina was sprayed on the precursor aluminum alloy preheated to 140-160°C to a thickness of 90-100 μm under the conditions of sandblasting pressure of 0.4-0.6 MPa, spraying distance of 115-125 mm, and powder feeding rate of 15-25 g / min, and then dried at 115-125°C for 1-3 h. The modified nano-alumina was then ultrasonically immersed in a functional polysiloxane solution for 4-6 min, taken out, allowed to stand at 20-30°C for 25-35 min, and dried at 145-155°C for 8-10 h to obtain a wear-resistant aluminum alloy material for smart watches.

3. The preparation process of a wear-resistant aluminum alloy material for a smart watch according to claim 2, characterized in that: The refining agent in step (2) is obtained by mixing potassium chloride, sodium chloride and sodium hexafluoroaluminate in a mass ratio of 1:0.64:0.

49.

4. The preparation process of a wear-resistant aluminum alloy material for a smart watch according to claim 2, characterized in that: The reaction equation of the polysiloxane precursor in step (3) is: 。 5. The preparation process of a wear-resistant aluminum alloy material for a smart watch according to claim 2, characterized in that: The reaction equation of the functional polysiloxane in step (3) is: 。 6. The preparation process of a wear-resistant aluminum alloy material for a smart watch according to claim 2, characterized in that: The porous silver-loaded nano-alumina in step (4) is prepared by mixing aluminum isopropoxide and deionized water in a mass ratio of 1:2, stirring at 85°C and 150 rpm for 60 min, adding a 1 mol / L nitric acid solution of 0.4 times the mass of aluminum isopropoxide, heating to 100°C for aging for 7 h, distilling at 85°C for 1 h, dropping the ball into an oil-ammonia column with a dropper, and pouring out to obtain a gel ball; washing the gel ball with isopropanol for 4 times, standing at 25°C for 24 h, and then drying at 110°C for 8 h, moving it into a muffle furnace, heating to 600°C at 3°C / min and calcining for 4 h, taking it out and naturally cooling it to room temperature, immersing it in a 25 g / L silver nitrate solution for 2 h, filtering it, washing it with anhydrous ethanol for 4 times, drying it at 75°C for 11 h, and calcining it at 300°C for 2 h.

7. The preparation process of a wear-resistant aluminum alloy material for a smart watch according to claim 2, characterized in that: The reaction equation of the pre-modified nano-alumina in step (4) is: 。 8. The process for preparing a wear-resistant aluminum alloy material for a smart watch according to claim 2, characterized in that: The reaction equation for the modified nano-alumina in step (4) is: 。 9. The preparation process of a wear-resistant aluminum alloy material for a smart watch according to claim 2, characterized in that: The functional polysiloxane solution in step (5) is obtained by mixing the functional polysiloxane and an ethanol solution having a volume fraction of 75% in a mass ratio of 1:5.

Citation Information

Patent Citations

  • Inorganic-organic coating composite material for nodular cast iron pipe and preparation method of inorganic-organic coating composite material

    CN114231171A

  • Continuous production process of alkoxy silane

    CN114479085A

  • Silicified steel-aluminum material

    CN116121603A

  • Preparation process of electromagnetic wire for wind power generation

    CN118762886A