Preparation method of high-temperature-resistant titanium alloy valve

By adding specific elements and process to the titanium alloy, titanium alloy valves with excellent mechanical properties are prepared, which solves the problem of insufficient mechanical properties of titanium alloy valves in high temperature environments, meets the usage requirements of HPD diesel engines, and improves the engine speed and power density.

CN119040691APending Publication Date: 2024-11-29CHINA WEAPON SCI ACADEMY NINGBO BRANCH
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410949568.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing titanium alloy valves lack mechanical properties in high temperature environments, making it difficult to meet the requirements of HPD diesel engines, and their large weight limits the engine's speed and power density.

Method used

Develop a high-temperature titanium alloy containing Al, Mo, Sn, Zr, B, Si, Nb, Y elements using the principle of multiple small amounts of alloying, and through specific preparation processes, including smelting, billet opening and forging, and bar material modification. titanium alloy valves with excellent mechanical properties were prepared by using diameter, machining, electric upsetting forging, heat treatment and PVD surface treatment.

Benefits of technology

It has achieved the improvement of the high temperature, tensile strength and elongation of the titanium alloy valve, and has excellent mechanical properties, oxidation resistance and wear resistance. It meets the use requirements of HPD diesel engines, and reduces the weight of the valve and improves the The engine's ultimate speed and power density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040691A_ABST
    Figure CN119040691A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant titanium alloy and a manufacturing method of a high-temperature-resistant titanium alloy valve, and the high-temperature-resistant titanium alloy comprises the following components in percentage by weight: 5.0-6.5% of Al, 0.8-1.8% of Mo, 2.0-3.0% of Sn, 4.5-6.5% of Zr, 0.5-1.5% of Nb, 0.3-0.5% of B, 0.1-0.3% of Si, 0.1-0.3% of Y and the balance of titanium and inevitable impurities, and the weight percentage of the impurities is less than or equal to 0.1%. The manufacturing method of the high-temperature-resistant titanium alloy air valve comprises the steps of burdening, smelting, cogging and precision forging, bar diameter changing, machining, electric upsetting die forging forming, finish machining and PVD treatment on the surface of the air valve. The titanium alloy valve prepared from the high-temperature-resistant titanium alloy has obdurability, high temperature resistance, oxidation resistance and wear resistance after being subjected to surface treatment, and can meet the use requirements of an HPD diesel engine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal alloys, and in particular to a high-temperature resistant titanium alloy and a method for preparing a high-temperature resistant titanium alloy valve. Background Art

[0002] The valve is an important core component of the engine. The function of the valve is to input air into the engine and discharge the exhaust gas after combustion. The valve is one of the bottlenecks in the development of HPD diesel engines. The main technical requirements are as follows: (1) The long-term service temperature of the valve is about 760℃, and it can work stably under load and the service conditions are extremely harsh; (2) High mechanical load requires the valve material to have high strength and high fatigue resistance; (3) High thermal load requires the valve to have high heat resistance; (4) High reciprocating motion requires the valve to have high wear resistance and impact resistance. Titanium alloy valves have good service performance in terms of lightweight, high temperature fatigue resistance, wear resistance and impact resistance, and are the preferred solution for the development of high power density diesel engines.

[0003] The Ni80 valves originally used in HPD diesel engines, despite their high density, exhibited large mass inertia in reciprocating motion, which limited the engine speed, thereby reducing the power density of the diesel engine by 6% to 8%. In contrast, titanium alloy valves have a significant advantage in weight, and their mass is 40% to 50% lighter than Ni80 valves. This improvement not only increases the diesel engine's maximum speed by up to 20%, but also makes the demand for titanium alloy valves particularly urgent for the development of high-power-density diesel engines.

[0004] However, with the continuous improvement of engine performance requirements, the use temperature and performance indicators of titanium alloy materials are also facing higher challenges. In order to meet this demand, it is urgent to develop high-temperature resistant titanium alloy materials that can work stably for a long time in an extreme high temperature environment above 600°C and have better mechanical properties. At the same time, it is also necessary to explore the corresponding preparation process to ensure that these high-performance titanium alloys can be successfully used in the manufacture of valves. Summary of the invention

[0005] The first technical problem to be solved by the present invention is to provide a high-temperature resistant titanium alloy with better mechanical properties in view of the above-mentioned technical status quo.

[0006] The second technical problem to be solved by the present invention is to provide a method for preparing high-temperature resistant titanium alloy valves using the aforementioned high-temperature resistant titanium alloy in response to the above-mentioned technical status quo, so that the prepared high-temperature resistant titanium alloy valves can meet the use requirements of HPD diesel engines.

[0007] The technical solution adopted by the present invention to solve the first technical problem mentioned above is: a high temperature resistant titanium alloy, characterized in that it contains the following components in weight percentage, Al: 5.0-6.5%, Mo: 0.8-1.8%, Sn: 2.0-3.0%, Zr: 4.5-6.5%, Nb: 0.5-1.5%, B: 0.3-0.5%, Si: 0.1-0.3%, Y: 0.1-0.3%, and the rest are titanium and unavoidable impurities, and the impurity content is ≤0.1%.

[0008] Furthermore, the impurities include Fe, and the weight percentage of Fe is ≤0.05%.

[0009] The high temperature resistant Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y titanium alloy of the present invention adopts the principle of multi-element and small amount alloying. On the basis of Ti-Al-Sn-Zr-Mo-Si, a high melting point metal Nb element is added, and trace amounts of Y and B elements are added, thereby ultimately improving the comprehensive mechanical properties of the titanium alloy and ensuring that the alloy has good processing performance.

[0010] Al and B elements are α stabilizers of titanium alloys, which can increase the β transformation temperature and expand the α phase area. Adding Al elements to titanium alloys can improve room temperature and high temperature strength, reduce the melting point of the alloy, reduce the density, improve oxidation resistance and hot workability, but when the Al content is ≥7%, it is easy to form a brittle α2 (Ti3Al) phase. The optimized design Al content is 5.0-6.5%. Adding a small amount of B elements can refine the grains and improve the performance of the alloy. The optimized design B content is 0.1-0.3%.

[0011] Mo, Si, and Fe are β-stabilizing elements, which can reduce the β transformation temperature and expand the β phase area; Mo element is infinitely dissolved in the β phase, and its solubility in α titanium at 600℃ is 0.8%. It can significantly improve the room temperature and high temperature strength through quenching and aging, increase hardenability, and improve the thermal stability of Cr or Fe alloys. The optimal design of Mo content is 2.0-3.0%. Si element can significantly improve the strength of the alloy and improve creep resistance; above 860℃, α titanium is dissolved at 0.45%, and after cooling, β phase titanium alloy precipitates α phase + high temperature phase Ti5Si3, but generally does not exceed 0.5%, and the optimal design of Si content is 0.1-0.3%; Fe element is one of the strongest β-stabilizing elements, but its thermal stability is not good, and segregation is easy to occur during smelting, and the Fe content is controlled to be ≤0.05.

[0012] Sn and Zr are neutral elements, weak strengthening agents, which can increase the recrystallization temperature of titanium alloy, improve the process plasticity of Ti-Al binary titanium alloy, suppress the ω phase, reduce the sensitivity of hydrogen embrittlement, and optimize the design of Sn content to 2.0-3.0%. The atomic size of Zr is very close to that of Ti, and it can be infinitely dissolved in the α phase and β phase, with a strong strengthening effect, but its plasticity will gradually deteriorate. When the Zr content is too high, granular substances will precipitate along the original β grain boundary. The optimized design of Zr content is 4.5-6.5%.

[0013] The addition of high melting point Nb element has a great influence on titanium alloy. Nb element can improve the oxidation resistance of the alloy through solid solution strengthening. The optimized design Nb content is 0.5-1.5%.

[0014] Y element can significantly improve the plasticity of titanium alloy by strengthening grain boundaries and preventing intergranular corrosion; it can also react with O, H, N, etc. in the alloy to form different types of compounds, among which the oxide produced with O has a higher melting point and is relatively stable under high temperature conditions, which can significantly improve the high-temperature mechanical properties of the alloy. The increase in the Y element content first increases and then decreases the density, hardness, strength and plasticity of titanium alloy, so the optimized design of Y content is 0.1-0.3%.

[0015] The technical solution adopted by the present invention to solve the second technical problem is: a method for preparing a high temperature resistant titanium alloy valve, characterized in that it is made of the above-mentioned high temperature resistant titanium alloy and comprises:

[0016] Step 1: Mixing ingredients: weigh the corresponding metals and master alloys according to the weight percentage of each component;

[0017] Step 2, smelting: heating the raw materials prepared in step 1 from low to high melting points, putting them into a crucible to melt and smelt them into an alloy ingot of the high temperature resistant titanium alloy;

[0018] Step 3: Opening and forging: The alloy ingot obtained in step 2 is open-forged and forged into titanium alloy bars;

[0019] Step 4: Re-diametering the bar: rolling the titanium alloy bar obtained in step 3 into a bar blank with a smaller diameter;

[0020] Step 5: Machining: peel the bar blank from step 4, and then machine it into a bar with a diameter suitable for forming into a valve;

[0021] Step 6: Preforming: The rods in step 5 are made into titanium alloy valve blanks by using electric upsetting preforming and die forging process;

[0022] Step 7: Heat treatment: subjecting the titanium alloy valve obtained in step 6 to solution treatment and aging heat treatment in sequence;

[0023] Step 8: Finishing: Finish the valve blank into valve products according to design requirements;

[0024] Step nine, PVD treatment of the valve surface: pre-cleaning, furnace loading, plasma cleaning, sputtering coating are performed in sequence, and finally the heating is turned off, and after cooling to room temperature, the furnace is opened and taken out to obtain the high-temperature resistant titanium alloy valve.

[0025] Preferably, the step 2, smelting: adopting a vacuum consumable arc furnace for smelting, placing pure aluminum ingots, aluminum-molybdenum master alloys, aluminum-zirconium master alloys, aluminum-niobium master alloys, aluminum-titanium-boron master alloys, aluminum-silicon master alloys, aluminum-yttrium master alloys, pure tin ingots and sponge titanium in order from low to high melting points of the alloys into a water-cooled copper crucible preheated to 330-360°C, heating and melting, and smelting 3-4 times under argon protection.

[0026] Preferably, the step three is blanking and fine forging: an anti-oxidation coating is sprayed on the surface of the alloy ingot, and then blanking and forging are performed at 950°C to 1150°C. The diameter of the first forging is 50 mm, the insulation temperature is 950 to 1050°C, and the insulation time is 0.5 to 1h. The diameter of the second forging is 30 mm, the insulation temperature is 850 to 950°C, and the insulation time is 1 to 2h. Then, the titanium alloy bar with a diameter of 20 mm is finely forged through a brake tube, and the fine forging temperature is 900 to 1000°C.

[0027] Preferably, in step 4, re-diametering the rod: the titanium alloy rod obtained in step 3 is kept in a high-temperature box-type resistance furnace for 1 to 2 hours at a temperature of 930 to 970°C, and is rolled to a diameter of 14 mm in the first pass and to a diameter of 10 mm in the second pass.

[0028] Preferably, in step six, electric upsetting die forging: the titanium alloy valve is preformed by electric upsetting and the blank is made by die forging. The electric upsetting is performed by a fully CNC forming machine, and the forming temperature is measured and recorded in real time. The forging is performed by a fully CNC screw press, and the forming temperature is within the range of 950 to 1100°C.

[0029] Preferably, the step seven, heat treatment: the titanium alloy valve obtained in step six is ​​subjected to solution heat treatment + aging heat treatment process in sequence, the solution heat treatment temperature is 950-1050°C, the holding time is 1-2 hours, and the cooling method is air cooling; the aging temperature is 680-780°C, the holding time is 5-6 hours, and the cooling method is air cooling.

[0030] Preferably, the step nine, PVD treatment of the valve surface: 1) Pre-cleaning: firstly, ultrasonically clean the workpiece, then use 0.5-0.7Mpa pressure to blow sand to clean the surface passivation layer, then ultrasonically clean it, and then blow dry it with compressed air; 2) Furnace loading: use specific tooling to clamp the product and put it into the vacuum chamber to reduce the obstruction surface and ensure uniform coating of the product; 3) Plasma cleaning: firstly, plasma clean the workpiece; 4) Sputtering coating: the target material is Cr target, the gas is nitrogen and / or argon, and the background vacuum degree reaches 5.0x10 -3 Pa, uniformly heat up to 400-600°C at a rate of 100-300°C / h, and maintain this temperature until the coating is completed, and perform vapor deposition on the product; 5) Turn off the heating, cool to room temperature, open the furnace and take out the workpiece.

[0031] Preferably, the step nine, PVD treatment of the valve surface: when sputtering coating, first clean the substrate, the sputtering time is 10 to 30 minutes, and 100 sccm of argon is used; then sputter Cr, the sputtering current is 2 to 4A, the sputtering time is 30 to 60 minutes, and 100 sccm of argon is used; then sputter Cr, the sputtering current is 2 to 4A, the sputtering time is 60 to 120 minutes, and 25 sccm of argon and 75 sccm of nitrogen are used; finally, sputter Cr, the sputtering current is 4 to 6A, the sputtering time is 180 to 240 minutes, and 25 sccm of argon and 75 sccm of nitrogen are used.

[0032] Compared with the prior art, the advantages of the present invention are:

[0033] (1) The present invention develops a new type of high-temperature resistant titanium alloy with excellent matching of strength, toughness and thermal stability through first-principles calculation, element alloying and microalloying, Al and Mo equivalent design, rare earth element addition and other methods; (2) The Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high-temperature resistant titanium alloy prepared by the present invention using the principle of multi-element and small amount alloying is an α+β dual-state structure, the equiaxed primary α phase improves the room temperature plasticity of the alloy, and the β transformation structure adjusts the high-temperature strength, so that the room temperature tensile strength reaches more than 1050MPa, and the elongation reaches more than 16%; the 650℃ tensile strength reaches more than 650MPa, and the elongation reaches more than 18%. (3) The titanium alloy valve prepared by the Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high-temperature resistant titanium alloy has excellent mechanical properties (strength, toughness and high temperature resistance), oxidation resistance, and wear resistance after surface treatment, which can meet the use requirements of HPD diesel engines. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A high temperature resistant titanium alloy valve blank manufactured according to an embodiment of the present invention;

[0035] Figure 2 The finished product of the high temperature resistant titanium alloy valve is obtained according to the embodiment of the present invention;

[0036] Figure 3 This is the microstructure of the high temperature resistant titanium alloy after deformation and heat treatment according to an embodiment of the present invention. DETAILED DESCRIPTION

[0037] The following is a further detailed description of the implementation examples of the present invention.

[0038] Example 1

[0039] The Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high temperature resistant titanium alloy in this embodiment contains the following components in weight percentage, Al: 5.0%, Mo: 0.8%, Sn: 2%, Zr: 4.5%, Nb: 0.5%, B: 0.3%, Si: 0.1%, Y: 0.1%, and the rest are titanium and unavoidable impurities, and the impurity content is ≤0.1%.

[0040] The preparation process of the Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high temperature resistant titanium alloy valve in this embodiment is as follows:

[0041] Material preparation - smelting - blanking and precision forging - bar diameter change - machining - electric upsetting die forging - precision machining - valve surface PVD treatment.

[0042] ① Ingredients: weigh pure aluminum ingots, aluminum-molybdenum master alloys, aluminum-zirconium master alloys, aluminum-niobium master alloys, aluminum-titanium-boron master alloys, aluminum-silicon master alloys, aluminum-yttrium master alloys, pure tin ingots and sponge titanium according to the weight percentage of each component.

[0043] ② Melting: Use a vacuum consumable arc furnace to melt pure aluminum ingots, aluminum-molybdenum master alloys, aluminum-zirconium master alloys, aluminum-niobium master alloys, aluminum-titanium-boron master alloys, aluminum-silicon master alloys, aluminum-yttrium master alloys, pure tin ingots and sponge titanium in order from low to high melting points of the alloys into a water-cooled copper crucible preheated to 330-360°C, and melt them three times under argon protection.

[0044] ③ Open forging: Spray anti-oxidation coating on the surface of the alloy ingot, then open forging is carried out at 950℃. The first forging process produces a diameter of 50mm (holding temperature is 950℃, holding time is 0.5h), and the second forging process produces a diameter of 30mm (holding temperature is 850℃, holding time is 1h), and then it is finely forged into a titanium alloy bar with a size of φ20mm through a brake tube (fine forging temperature is 900℃).

[0045] ④ Rod diameter reshaping: The titanium alloy rod obtained in step ③ is kept in a high-temperature box-type resistance furnace for 1 hour at a holding temperature of 930°C. The first pass is rolled into a diameter of φ14 mm, and the second pass is rolled into a diameter of φ10 mm.

[0046] ⑤ Machining: The bar blank is peeled and then machined into a bar with a diameter of 8.6mm*260mm.

[0047] ⑥Electric upsetting die forging: Titanium alloy valves are preformed by electric upsetting and die forging. Electric upsetting uses a fully CNC forming machine, and the forming temperature is measured and recorded in real time. Forging uses a fully CNC screw press, and the forming temperature is within the range of 950-1100℃. The valve blanks are as follows: Figure 1 shown.

[0048] ⑦ Heat treatment: The titanium alloy valve obtained in step ⑥ is subjected to solution + aging heat treatment process in sequence, with the solution treatment temperature being 950°C, the holding time being 1 hour, and the cooling method being air cooling; the aging temperature being 680°C, the holding time being 5 hours, and the cooling method being air cooling.

[0049] ⑧Fine machining: According to the design requirements, the valve products are finely processed on CNC machine tools and other equipment.

[0050] ⑨ PVD treatment of valve surface: 1) Pre-cleaning: First, ultrasonically clean the workpiece, then use 0.5Mpa pressure to blow sand to clean the surface passivation layer, then ultrasonically clean it, and then blow it dry with compressed air; 2) Furnace loading: Use specific tooling to clamp the product and put it into the vacuum chamber to reduce the obstruction surface and ensure uniform coating of the product; 3) Plasma cleaning: First, plasma clean the workpiece; 4) Sputtering coating: Cr target is used as the target material, nitrogen and argon are used as the gas, and the background vacuum degree reaches 5.0x10 -3 Pa, the temperature is raised to 400°C at a rate of 100°C / h, and the temperature is maintained until the coating is completed. The product is subjected to vapor deposition. The process parameters are shown in Table 1; 5) Turn off the heating, cool to room temperature, open the furnace and take out the workpiece. The valve product is as follows Figure 2 shown.

[0051] Table 1 PVD treatment process for valve surface

[0052]

[0053] Example 2

[0054] The Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high temperature resistant titanium alloy in this embodiment contains the following components in weight percentage, Al: 6.0%, Mo: 1.2%, Sn: 2.5%, Zr: 5.0%, Nb: 1.0%, B: 0.4%, Si: 0.2%, Y: 0.2%, and the rest are titanium and unavoidable impurities, and the impurity content is ≤0.1%.

[0055] The preparation process of the Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high temperature resistant titanium alloy valve in this embodiment is as follows:

[0056] Material preparation - smelting - blanking and precision forging - bar diameter change - machining - electric upsetting die forging - precision machining - valve surface PVD treatment.

[0057] ① Ingredients: weigh pure aluminum ingots, aluminum-molybdenum master alloys, aluminum-zirconium master alloys, aluminum-niobium master alloys, aluminum-titanium-boron master alloys, aluminum-silicon master alloys, aluminum-yttrium master alloys, pure tin ingots and sponge titanium according to the weight percentage of each component.

[0058] ② Melting: Use a vacuum consumable arc furnace to melt pure aluminum ingots, aluminum-molybdenum master alloys, aluminum-zirconium master alloys, aluminum-niobium master alloys, aluminum-titanium-boron master alloys, aluminum-silicon master alloys, aluminum-yttrium master alloys, pure tin ingots and sponge titanium in order from low to high melting points of the alloys into a water-cooled copper crucible preheated to 330-360°C, and melt them 4 times under argon protection.

[0059] ③ Open forging: Spray anti-oxidation coating on the surface of the alloy ingot, then open forging is carried out at 1050℃. The first forging process produces a diameter of 50mm (holding temperature is 950℃, holding time is 1h), and the second forging process produces a diameter of 30mm (holding temperature is 900℃, holding time is 1.5h), and then it is finely forged into a titanium alloy bar with a size of φ20mm through a brake tube (fine forging temperature is 950℃).

[0060] ④ Rod diameter reshaping: The titanium alloy rod obtained in step ③ is kept in a high-temperature box-type resistance furnace for 1.5 hours at a holding temperature of 950°C. The first pass is rolled into a diameter of φ14 mm, and the second pass is rolled into a diameter of φ10 mm.

[0061] ⑤ Machining: The bar blank is peeled and then machined into a bar with a diameter of 8.6mm*260mm.

[0062] ⑥Electric upsetting die forging: Titanium alloy valves are preformed by electric upsetting and die forging. Electric upsetting uses a fully CNC forming machine to measure and record the forming temperature in real time. Forging uses a fully CNC screw press, and the forming temperature is within the range of 1000℃. The valve blank is Figure 1 shown.

[0063] ⑦ Heat treatment: The titanium alloy valve obtained in step ⑥ is subjected to solution + aging heat treatment process in sequence, with the solution treatment temperature being 1020°C, the holding time being 1.5 hours, and the cooling method being air cooling; the aging temperature being 720°C, the holding time being 5.5 hours, and the cooling method being air cooling.

[0064] ⑧Fine machining: According to the design requirements, the valve products are finely processed on CNC machine tools and other equipment.

[0065] ⑨ PVD treatment of valve surface: 1) Pre-cleaning: First, ultrasonically clean the workpiece, then use 0.5-0.7Mpa pressure to blow sand to clean the surface passivation layer, then ultrasonically clean it, and then blow it dry with compressed air; 2) Furnace loading: Use specific tooling to clamp the product and put it into the vacuum chamber to reduce the obstruction surface and ensure uniform coating of the product; 3) Plasma cleaning: First, plasma clean the workpiece; 4) Sputtering coating: Cr target is used as the target material, nitrogen and argon are used as the gas, and the background vacuum degree reaches 5.0x10 - 3 Pa, the temperature is raised to 500°C at a rate of 200°C / h, and the temperature is maintained until the coating is completed, and the product is subjected to vapor deposition. The process parameters are shown in Table 2; 5) Turn off the heating, cool to room temperature, open the furnace and take out the workpiece. The finished valve is as follows Figure 2 shown.

[0066] Table 2 PVD treatment process of valve surface

[0067]

[0068]

[0069] Example 3

[0070] The Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high temperature resistant titanium alloy in this embodiment contains the following components in weight percentage, Al: 6.5%, Mo: 1.6%, Sn: 3.0%, Zr: 6.5%, Nb: 1.5%, B: 0.5%, Si: 0.3%, Y: 0.3%, and the rest are titanium and unavoidable impurities, and the impurity content is ≤0.1%.

[0071] The preparation process of the Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high temperature resistant titanium alloy valve in this embodiment is as follows:

[0072] Material preparation - smelting - blanking and precision forging - bar diameter change - machining - electric upsetting die forging - precision machining - valve surface PVD treatment.

[0073] ① Ingredients: weigh pure aluminum ingots, aluminum-molybdenum master alloys, aluminum-zirconium master alloys, aluminum-niobium master alloys, aluminum-titanium-boron master alloys, aluminum-silicon master alloys, aluminum-yttrium master alloys, pure tin ingots and sponge titanium according to the weight percentage of each component.

[0074] ② Melting: Use a vacuum consumable arc furnace to melt pure aluminum ingots, aluminum-molybdenum master alloys, aluminum-zirconium master alloys, aluminum-niobium master alloys, aluminum-titanium-boron master alloys, aluminum-silicon master alloys, aluminum-yttrium master alloys, pure tin ingots and sponge titanium in order from low to high melting points of the alloys into a water-cooled copper crucible preheated to 330-360°C, and melt them three times under argon protection.

[0075] ③ Open forging: Spray anti-oxidation coating on the surface of the alloy ingot, then open forging is carried out at 1150℃. The first forging process produces a diameter of 50mm (holding temperature is 1050℃, holding time is 1h), and the second forging process produces a diameter of 30mm (holding temperature is 950℃, holding time is 2h), and then it is finely forged into a titanium alloy bar with a size of φ20mm through a brake tube (fine forging temperature is 1000℃).

[0076] ④ Rod diameter reshaping: The titanium alloy rod obtained in step ③ is kept in a high-temperature box-type resistance furnace for 2 hours at a holding temperature of 970°C. The first pass is rolled into a diameter of φ14 mm, and the second pass is rolled into a diameter of φ10 mm.

[0077] ⑤ Machining: The bar blank is peeled and then machined into a bar with a diameter of 8.6mm*260mm.

[0078] ⑥Electric upsetting die forging: Titanium alloy valves are preformed by electric upsetting and die forging. Electric upsetting uses a fully CNC forming machine to measure and record the forming temperature in real time. Forging uses a fully CNC screw press, and the forming temperature is within the range of 1100°C. The valve blank is Figure 1 shown.

[0079] ⑦ Heat treatment: The titanium alloy valve obtained in step ⑥ is subjected to solution + aging heat treatment process in sequence, the solution treatment temperature is 1050°C, the holding time is 2 hours, and the cooling method is air cooling; the aging temperature is 780°C, the holding time is 6 hours, and the cooling method is air cooling.

[0080] ⑧Fine machining: According to the design requirements, the valve products are finely processed on CNC machine tools and other equipment.

[0081] ⑨ PVD treatment of valve surface: 1) Pre-cleaning: First, ultrasonically clean the workpiece, then use 0.7Mpa pressure to blow sand to clean the surface passivation layer, then ultrasonically clean it, and then blow it dry with compressed air; 2) Furnace loading: Use specific tooling to clamp the product and put it into the vacuum chamber to reduce the obstruction surface and ensure uniform coating of the product; 3) Plasma cleaning: First, plasma clean the workpiece; 4) Sputtering coating: Cr target is used as the target material, nitrogen and argon are used as the gas, and the background vacuum degree reaches 5.0x10 -3 Pa, the temperature is raised to 600℃ at a uniform rate of 300℃ / h, and the temperature is maintained until the coating is completed, and the product is subjected to vapor deposition. The process parameters are shown in Table 3; 5) Turn off the heating, cool to room temperature, open the furnace and take out the workpiece. The finished valve is as follows Figure 2 shown.

[0082] Table 3 PVD treatment process of valve surface

[0083]

[0084] The Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y high temperature resistant titanium alloy prepared by the above three embodiments using the principle of multi-element and small amount alloying is an α+β dual state structure. Figure 3 As shown, the equiaxed primary α phase improves the room temperature plasticity of the alloy, and the β transformation structure adjusts the high temperature strength. The mechanical properties and wear resistance parameters are shown in Table 4. The room temperature tensile strength reaches more than 1050MPa, and the elongation reaches more than 16%; the 650℃ tensile strength reaches more than 650MPa, and the elongation reaches more than 18%.

[0085] Table 4 Mechanical properties and wear resistance of Ti-Al-Sn-Zr-Mo-B-Si-Nb-Y titanium alloy in different implementation cases

[0086]

Claims

1. A high temperature resistant titanium alloy, It is characterized in that The invention comprises the following components in weight percentage: Al: 5.0-6.5%, Mo: 0.8-1.8%, Sn: 2.0-3.0%, Zr: 4.5-6.5%, Nb: 0.5-1.5%, B: 0.3-0.5%, Si: 0.1-0.3%, Y: 0.1-0.3%, and the rest are titanium and unavoidable impurities, and the weight percentage of the impurities is ≤0.1%.

2. The high temperature resistant titanium alloy according to claim 1, It is characterized in that The impurities include Fe, and the weight percentage of Fe is ≤0.05%.

3. A method for preparing a high temperature resistant titanium alloy valve, It is characterized in that Made of the high temperature resistant titanium alloy according to claim 1 or 2, comprising in sequence: Step 1: Mixing ingredients: weigh the corresponding metals and master alloys according to the weight percentage of each component; Step 2, smelting: heating the raw materials prepared in step 1 from low to high melting points, putting them into a crucible to melt and smelt them into an alloy ingot of the high temperature resistant titanium alloy; Step 3: Opening and forging: The alloy ingot obtained in step 2 is open-forged and forged into titanium alloy bars; Step 4: Re-diametering the bar: rolling the titanium alloy bar obtained in step 3 into a bar blank with a smaller diameter; Step 5: Machining: peel the bar blank from step 4, and then machine it into a bar with a diameter suitable for forming into a valve; Step 6: Preforming: The rod material in step 5 is made into a titanium alloy valve blank by using electric upsetting preforming and die forging process; Step 7: Heat treatment: subjecting the titanium alloy valve obtained in step 6 to solution treatment and aging heat treatment in sequence; Step 8: Finishing: Finish the valve blank into valve products according to design requirements; Step nine, PVD treatment of the valve surface: pre-cleaning, furnace loading, plasma cleaning, sputtering coating are performed in sequence, and finally the heating is turned off, and after cooling to room temperature, the furnace is opened and taken out to obtain the high-temperature resistant titanium alloy valve.

4. The method for preparing a high temperature resistant titanium alloy valve according to claim 3, It is characterized in that The second step is smelting: using a vacuum consumable arc furnace for smelting, placing pure aluminum ingots, aluminum-molybdenum master alloys, aluminum-zirconium master alloys, aluminum-niobium master alloys, aluminum-titanium-boron master alloys, aluminum-silicon master alloys, aluminum-yttrium master alloys, pure tin ingots and sponge titanium in order from low to high melting points of the alloys into a water-cooled copper crucible preheated to 330-360° C., heating and melting, and smelting 3-4 times under argon protection.

5. The method for preparing a high temperature resistant titanium alloy valve according to claim 4, It is characterized in that The step three is blanking and fine forging: an anti-oxidation coating is sprayed on the surface of the alloy ingot, and then blanking and forging are performed at 950°C to 1150°C. The first forging process results in a diameter of 50 mm, a holding temperature of 950°C to 1050°C, and a holding time of 0.5 to 1h. The second forging process results in a diameter of 30 mm, a holding temperature of 850°C to 950°C, and a holding time of 1 to 2h. The titanium alloy bar is then finely forged through a brake tube into a titanium alloy bar with a diameter of 20 mm, and the fine forging temperature is 900 to 1000°C.

6. The method for preparing a high temperature resistant titanium alloy valve according to claim 5, It is characterized in that The fourth step is to change the diameter of the rod: the titanium alloy rod obtained in the third step is kept in a high temperature box-type resistance furnace for 1 to 2 hours at a temperature of 930 to 970° C. The first rolling process is used to roll the rod to a diameter of 14 mm and the second rolling process is used to roll the rod to a diameter of 10 mm.

7. The method for preparing a high temperature resistant titanium alloy valve according to claim 6, It is characterized in that The step six, electric upsetting die forging: the titanium alloy valve is preformed by electric upsetting, and the die forging process is used. The electric upsetting adopts a fully CNC forming machine, and the forming temperature is measured and recorded in real time; the forging adopts a fully CNC screw press, and the forming temperature is within the range of 950-1100°C.

8. The method for preparing a high temperature resistant titanium alloy valve according to claim 7, It is characterized in that The step seven, heat treatment: the titanium alloy valve obtained in step six is ​​subjected to solution + aging heat treatment process in sequence, the solution treatment temperature is 950-1050°C, the holding time is 1-2 hours, and the cooling method is air cooling; the aging temperature is 680-780°C, the holding time is 5-6 hours, and the cooling method is air cooling.

9. The method for preparing a high temperature resistant titanium alloy valve according to claim 8, It is characterized in that Step 9: PVD treatment of valve surface: 1) Pre-cleaning: First, ultrasonically clean the workpiece, then use 0.5-0.7Mpa pressure to blow sand to clean the surface passivation layer, then ultrasonically clean it, and then blow it dry with compressed air; 2) Furnace loading: Use specific tooling to clamp the product and put it into the vacuum chamber to reduce the obstruction surface and ensure uniform coating of the product; 3) Plasma cleaning: First, plasma clean the workpiece; 4) Sputtering coating: The target material is Cr target, and the gas is nitrogen and / or argon. The background vacuum degree reaches 5.0x10 -3 Pa, uniformly heat up to 400-600°C at a rate of 100-300°C / h, and maintain this temperature until the coating is completed, and perform vapor deposition on the product; 5) Turn off the heating, cool to room temperature, open the furnace and take out the workpiece.

10. The method for preparing a high temperature resistant titanium alloy valve according to claim 9, It is characterized in that The step nine, PVD treatment of the valve surface: when sputtering coating, first clean the substrate, the sputtering time is 10 to 30 minutes, and 100 sccm of argon is used; then sputter Cr, the sputtering current is 2 to 4A, the sputtering time is 30 to 60 minutes, and 100 sccm of argon is used; then sputter Cr, the sputtering current is 2 to 4A, the sputtering time is 60 to 120 minutes, and 25 sccm of argon and 75 sccm of nitrogen are used; finally, sputter Cr, the sputtering current is 4 to 6A, the sputtering time is 180 to 240 minutes, and 25 sccm of argon and 75 sccm of nitrogen are used.

Citation Information

Cited By

  • Wear-resistant strengthening process for light titanium alloy gear

    CN119550005A

  • TiAl alloy valve blank and preparation method thereof

    CN120287009A

  • Ti al alloy valve blank and method of making

    CN120287009B

  • Preparation method for near-net forming of light high-temperature-resistant TiAl alloy valve

    CN120734333A