Preparation method of high-toughness and high-straightness flat rolled steel plate

Through specific steel composition and process flow, the problem of high toughness and high straightness of thin and wide-specification flat-rolled steel plates is solved, and flat-rolled steel plates with excellent performance and low cost are prepared, which are suitable for a variety of engineering manufacturing fields.

CN119040737APending Publication Date: 2024-11-29SD STEEL RIZHAO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410975861.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to meet the high toughness and high straightness requirements of thin and wide-size flat-rolled steel plates with thickness of 6-10mm and width >3600mm. The production process is high and the process is complicated, so there is difficulty in controlling the plate type and risk of production accidents. The problem.

Method used

Specific steel composition ratios are adopted (C: 0.050%-0.140%, Mn: 0.80%-1.80%, Si≤0.20%, Nb: 0.008%-0.050%, Ti: 0.008%-0.020%, Al≤0.035%, P≤0.015%, S:≤0.0030%) and process flow, including molten iron pretreatment, BOF steelmaking, LF refining, continuous casting, casting billet heating, rolling, cooling, straightening processes, controlling the casting billet outlet temperature and heating Time, one-stage rolling and water mist cooling are used to ensure the reasonable relationship between rolling temperature and deformation rate, and reduce the difficulty of temperature drop and plate type control.

Benefits of technology

Prepare a flat-rolled steel plate with simple composition and good microstructure uniformity, high toughness and high straightness. The yield strength is ≤440MPa, straightness is ≤3mm/m, and the impact force of -40℃ KV2 ≥140J, with excellent plasticity and Machining capability, short production cycle and low cost, suitable for a variety of engineering manufacturing fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040737A_ABST
    Figure CN119040737A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metallurgy, in particular to a preparation method of a high-toughness and high-straightness flat rolled steel plate. The flat rolled steel plate comprises the following chemical components in percentage by mass: 0.05%-0.14% of C, 0.8%-1.8% of Mn, less than or equal to 0.20% of Si, 0.008%-0.05% of Nb, 0.008%-0.02% of Ti, less than or equal to 0.035% of Al, less than or equal to 0.015% of P, less than or equal to 0.003% of S and the balance of Fe and other inevitable impurities. Meanwhile, 0.16% < = (% C) + (% Mn) / 6 < = 0.19%, and 0.045% < = (% Nb) + (% Al) + (% Ti) < = 0.070%; the preparation method of the flat rolled steel plate comprises the steps of molten iron pretreatment, smelting, refining, continuous casting, casting blank heating, rolling, cooling and straightening. The prepared flat rolled steel plate has high toughness and high straightness and is beneficial to popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a method for preparing a flat-rolled steel plate with high toughness and high flatness. Background Art

[0002] In the metallurgical industry, thin and wide flat-rolled steel plates (i.e. flat-rolled steel plates with low thickness and large width) have the advantages of fewer welding points and light weight. They are widely used in fields such as ships, bridges, and pipeline projects. They can reduce the dead weight of structural parts or equipment, reduce welding points and welding volume, and reduce welding difficulty and engineering costs.

[0003] In the existing production process of thin and wide flat-rolled steel plates, the production process of thin and wide flat-rolled steel plates with a thickness of 6-10mm and a width of >3600mm has the problem of greater difficulty in controlling the plate shape. Quality problems such as double-side waves and large and medium waves are prone to occur during the rolling process. There is even a risk of rolling through and causing production accidents during the rolling process.

[0004] At the same time, the existing production process of thin and wide flat-rolled steel plates with a thickness of 6-10mm and a width of >3600mm is difficult to meet the requirements of high toughness and high flatness at the same time. If high-temperature rolling is adopted to ensure the shape of thin and wide flat-rolled steel plates, coarse grains or mixed crystals are likely to occur in the steel plate structure during the rolling process, resulting in poor low-temperature toughness of thin and wide flat-rolled steel plates; and if low-temperature controlled rolling is adopted to prepare thin and wide flat-rolled steel plates in order to ensure high toughness requirements, the difficulty of plate shape control will be further increased, and the flatness of the obtained thin and wide flat-rolled steel plates will basically be above 8mm / m.

[0005] There are also methods in the prior art to improve the performance of thin and wide flat-rolled steel plates by adding precious metal elements, changing the production process, etc. For example, Chinese patent CN106544597A discloses an ultra-thin and ultra-wide steel plate for nuclear power pressure equipment and a manufacturing method thereof. The chemical composition of the steel is C: ≤0.20%; Si: ≤0.10%; Mn: 0.50%-1.80%; P: ≤0.008%; S: ≤0.003%; Ni: 0.20%-1.00%; Cr: 0.30%-0.80%; Cu: 0.10%-0.80%; Mo: ≤0.08%; Alt: ≤0.040%; N: ≤0.008%; rolling is carried out using a two-fire process and heat treatment is carried out using a normalizing process. However, in order to improve the performance of the steel plate in this technical solution, a large amount of precious alloy elements such as Cr, Cu, Ni, etc. are added to the steel raw materials, and the raw material cost of the steel is high; at the same time, two-fire rolling and normalizing heat treatment are also adopted, and the steel production process has many steps, complex technology, and high production cost.

[0006] Chinese patent CN113235010A discloses a method for preparing a thin-gauge steel plate with uniform performance for nuclear power, which is designed with low carbon, low silicon and a small amount of rare earth alloy components, and uses hot rollers, billet heating, and idle roller cooling water protection to control the plate shape, and uses normalizing and high-temperature stacking and slow cooling to improve the performance and shape of the steel plate, and successfully achieves mass production of 5.5-10.5mm steel plates. However, the addition of rare earth alloy components in this technical solution also greatly increases the cost of steel raw materials, and the use of hot rollers, normalizing, high-temperature stacking and slow cooling to ensure the plate shape and performance has many and complex processes, and the production cycle and cost are high. Summary of the invention

[0007] Aiming at the technical problems that the existing process for preparing thin and wide flat-rolled steel plates with a thickness of 6-10mm and a width of >3600mm is difficult to meet the requirements of high toughness and high flatness at the same time, and the high raw material cost, complicated process and high preparation cost of high-performance flat-rolled steel plates, the present invention provides a method for preparing flat-rolled steel plates with high toughness and high flatness. The prepared flat-rolled steel plates have simple composition, good microstructure uniformity, excellent plasticity and toughness as well as high flatness, excellent machining capability, low cost, and are conducive to promotion and application.

[0008] The technical solution of the present invention is: A method for preparing a flat-rolled steel plate with high toughness and high flatness, wherein the chemical composition mass percentage of the flat-rolled steel plate is C: 0.050%-0.140%, Mn: 0.80%-1.80%, Si≤0.20%, Nb: 0.008%-0.050%, Ti: 0.008%-0.020%, Al≤0.035%, P≤0.015%, S:≤0.0030%, and the rest is Fe and other inevitable impurities; At the same time, 0.16%≤(%C)+(%Mn) / 6≤0.19%, 0.045%≤(%Nb)+(%Al)+(%Ti)≤0.070%; The preparation steps of flat-rolled steel plates include: molten iron pretreatment, smelting, refining, continuous casting, billet heating, rolling, cooling, and straightening processes.

[0009] Furthermore, the thickness of the flat-rolled steel plate is 6-10mm, the width is >3600mm, and the length is <55m; the yield strength of the flat-rolled steel plate is ≤440MPa, the straightness is ≤3mm / m, and the -40℃ KV2 impact energy is ≥140J.

[0010] Furthermore, the smelting process adopts BOF steelmaking process.

[0011] Furthermore, the refining process adopts LF refining, and after LF refining, RH vacuum treatment is performed, and then a continuous casting process is performed.

[0012] Furthermore, the parameters of the ingot heating process are controlled as follows: ingot furnace discharge temperature 1200-1250°C, soaking time 20min≤30min, total heating time / H 1.3min / mm≤1.5min / mm, where H is ingot thickness.

[0013] Since thin and wide flat-rolled steel plates have many rolling passes, the heat dissipation is fast and the temperature drop is large during the rolling process. The internal and external temperature difference of the ingot is easily magnified on the thin and wide flat-rolled steel plates, resulting in low surface temperature and difficulty in plate shape control, resulting in large performance differences of the same plate and wave shape of the steel plate. The present invention controls the ingot furnace discharge temperature, soaking period time and total heating time. On the one hand, the internal and external temperature difference of the ingot when it is discharged from the furnace is small, basically controlled within 10°C, reducing the temperature difference at various parts of the steel plate, and achieving the purpose of reducing the difficulty of plate shape control; on the other hand, the high furnace discharge temperature and the high internal and external temperature of the ingot are matched, which is easy to deform by large pressure rolling in a single pass, reducing the number of rolling passes, reducing the temperature drop in the entire rolling process, and achieving the purpose of reducing the difficulty of plate shape control.

[0014] Furthermore, the billet is removed from the furnace and descaled by high-pressure water before rolling. The rolling is carried out in one stage and completed in the complete recrystallization zone. The first rolling temperature is satisfy =1027+483×(%C)+896×(%Ti)+373×(%Al)-353×(%Si)+6652×(%Nb)-432×SQRT(%Nb)+862×(%V)-232×SQRT(%V).

[0015] Calculate and select the appropriate temperature according to the actual composition of the billet ( ) for the first rolling pass is more conducive to reducing the temperature drop of the first rolling pass and reducing the difficulty of flat-rolled steel plate shape control.

[0016] Furthermore, the rolling temperature of each of the last 3-4 passes of the rolling process , Export thickness , deformation rate Satisfy 15≤ × / ≤25.

[0017] The last 3-4 passes of the rolling process are the key to plate shape control, which requires a reasonable relationship between the rolling temperature, the exit thickness of each pass, and the pass deformation rate, so as to achieve uniform longitudinal extension of the steel plate. Achieved high-speed deformation at high temperature, by controlling 15≤ × / ≤25 to achieve uniform deformation of the flat-rolled steel plate in the last 3-4 passes of the rolling process, thereby obtaining austenite grains of uniform size, preparing for the subsequent phase transformation to generate ferrite of uniform size.

[0018] Furthermore, the parameters of the cooling process are controlled as follows: the rolled piece is subjected to water mist cooling after rolling, and the temperature is cooled to 630-680°C.

[0019] The production of thin-gauge flat-rolled steel plates requires high temperature uniformity and high deformation uniformity. Water mist cooling has high cooling uniformity and low cooling intensity, which is conducive to the shape control of the flat-rolled steel plates. The temperature of the flat-rolled steel plates after cooling is 630-680℃, which is easy to straighten the plate shape.

[0020] The beneficial effects of the present invention are: The method for preparing a flat-rolled steel plate with high toughness and high flatness provided by the present invention adopts appropriate steel composition and suitable production process, so that the obtained flat-rolled steel plate has simple composition and good microstructure uniformity; the thickness of the flat-rolled steel plate is 6-10mm and the width is >3600mm, which meets the specification requirements of thin and wide flat-rolled steel plates; the yield strength of the flat-rolled steel plate is ≤440MPa, the flatness is ≤3mm / m, and the -40℃ KV2 impact energy is ≥140J. It has excellent plasticity and toughness as well as high flatness, and has excellent machining ability, and can be applied to equipment and engineering manufacturing fields such as welding of structural parts with high flatness requirements and pipe welding; the flat-rolled steel plate of the present invention has a simple production process, a short production cycle, and low cost, which is conducive to promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0022] Figure 1 This is the metallographic structure diagram of the flat-rolled steel plate obtained in Example 1.

[0023] Figure 2 This is the metallographic structure diagram of the flat-rolled steel plate obtained in Example 1. DETAILED DESCRIPTION

[0024] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0025] Example 1 A method for preparing a flat-rolled steel plate with high toughness and high flatness, wherein the chemical composition mass percentage of the flat-rolled steel plate is: C: 0.14%, Si: 0.23%, Mn: 1.25%, P: 0.014%, S: 0.003%, Al: 0.033%, Nb: 0.016%, Ti: 0.016%, and the rest is Fe and unavoidable impurities, and the preparation steps of the flat-rolled steel plate include molten iron pretreatment, smelting, refining, continuous casting, heating of ingot, rolling, cooling, and straightening processes; Among them, the smelting process adopts BOF steelmaking process, adopts molten iron pretreatment, and the final S content is 0.001%; ​​the converter adopts top and bottom double blowing, fully dephosphorizes, and the final phosphorus content is 0.005%. Argon is blown throughout the process, weak stirring, the slag surface is slightly turned over without being exposed, and lime and fluorite are used to make white slag; RH vacuum degree is 100pa, vacuum time is 10min; molten steel is calmed for 31min before tapping; The refining process adopts LF refining, and after LF refining, RH vacuum treatment is performed, and then a continuous casting process is performed to continuously cast into a 150mm×1820mm ingot, and then a ingot heating process is performed; The parameters of the billet heating process are as follows: billet out-of-furnace temperature 1232°C, soaking time 52 min, total heating time 225 min, total heating time / H=1.5 min / mm, H is billet thickness; The process of descaling and rolling of the ingot is as follows: the ingot is descaled by 31MPa high-pressure water after it is taken out of the furnace and then rolling begins. The rolling adopts one-stage rolling, with a total of 12 rolling passes, and the starting rolling temperature is 1118℃. × / =17, × / =24, × / =24; The parameters of the cooling process are controlled as follows: the rolled piece is cooled by water mist after rolling to a temperature of 660°C; The flat-rolled steel plate obtained in Example 1 has a specification of 6 mm×3700 mm×52 mm. The microstructure of the flat-rolled steel plate is shown in FIG. Figure 1 shown.

[0026] Example 2 A method for preparing a flat-rolled steel plate with high toughness and high flatness, wherein the chemical composition of the flat-rolled steel plate is C: 0.12%, Si: 0.16%, Mn: 1.08%, P: 0.012%, S: 0.003%, Al: 0.032%, Nb: 0.032%, Ti: 0.018%, and the rest is Fe and unavoidable impurities, and the preparation steps of the flat-rolled steel plate include molten iron pretreatment, smelting, refining, continuous casting, heating of ingots, rolling, cooling, and straightening processes; Among them, the smelting process adopts BOF steelmaking process, adopts molten iron pretreatment, and the final S content is 0.002%; the converter adopts top and bottom double blowing, fully dephosphorizes, and the final phosphorus content is 0.006%. Argon is blown throughout the process, weak stirring, the slag surface is slightly turned over without being exposed, and lime and fluorite are used to make white slag; RH vacuum degree is 100pa, vacuum time is 9min; molten steel is calmed for 28min before tapping; The refining process adopts LF refining, and after LF refining, RH vacuum treatment is performed, and then a continuous casting process is performed to continuously cast into a 150mm×1820mm ingot, and then a ingot heating process is performed; The parameters of the billet heating process are as follows: billet out-of-furnace temperature 1225°C, soaking time 48 min, total heating time 207 min, total heating time / H=1.38 min / mm, H is billet thickness; The process of descaling and rolling of the ingot is as follows: the ingot is descaled by 31MPa high pressure water after it is taken out of the furnace and then rolling begins. The rolling adopts one-stage rolling, with a total of 12 rolling passes, and the starting rolling temperature is 1166℃. × / =16, × / =16, × / =18; The parameters of the cooling process are controlled as follows: the rolled piece is cooled by water mist after rolling to a temperature of 673°C; The flat-rolled steel plate obtained in Example 2 has a specification of 10 mm×3980 mm×50 m.

[0027] Comparative Example 1 A method for preparing a flat-rolled steel plate, wherein the chemical composition of the flat-rolled steel plate is C: 0.14%, Si: 0.23%, Mn: 1.25%, P: 0.014%, S: 0.003%, Al: 0.033%, Nb: 0.016%, Ti: 0.016%, and the rest is Fe and unavoidable impurities, and the preparation steps of the flat-rolled steel plate include molten iron pretreatment, smelting, refining, continuous casting, heating of ingots, rolling, cooling, and straightening processes; Among them, the smelting process adopts BOF steelmaking process, adopts molten iron pretreatment, and the final S content is 0.002%; the converter adopts top and bottom double blowing, fully dephosphorizes, and the final phosphorus content is 0.010%. Argon is blown throughout the process, weak stirring, the slag surface is slightly turned over without being exposed, and lime and fluorite are used to make white slag; RH vacuum degree is 200pa, vacuum time is 7min; molten steel is calmed for 22min before tapping; The refining process adopts LF refining, and after LF refining, RH vacuum treatment is performed, and then a continuous casting process is performed to continuously cast into a 150mm×1820mm ingot, and then a ingot heating process is performed; The parameters of the billet heating process are controlled as follows: billet out of furnace temperature 1280°C; The process of descaling and rolling of the ingot is as follows: the ingot is descaled by 31MPa high-pressure water after it is taken out of the furnace and then rolling begins. The rolling adopts one-stage rolling, with a total of 10 rolling passes. The starting rolling temperature is 1187℃, and a large compression ratio rolling is carried out at high temperature. The final rolling temperature is 958℃. × / =16, × / =16, × / =27; The parameters of the cooling process are as follows: the rolled piece is cooled by water curtain after rolling to a temperature of 673°C; The flat-rolled steel plate obtained in Comparative Example 1 has a specification of 10 mm × 37000 mm × 50 mm. The microstructure of the flat-rolled steel plate is shown in FIG. Figure 2 shown.

[0028] The rolling process parameters of each embodiment and comparative example are shown in Table 1.

[0029] Table 1 Rolling process parameters

[0030] The flat-rolled steel plates prepared in each embodiment and comparative example were respectively subjected to mechanical property tests and low-temperature toughness tests, and the test results are shown in Tables 2 and 3.

[0031] Table 2 Mechanical properties test results of flat-rolled steel plates serial number Thickness / mm Yield strength / MPa Tensile strength / MPa Elongation after fracture A / % Straightness mm / m Example 1 6 398 565 27.5 2.8 Example 2 10 402 583 25.5 2.7 Comparative Example 1 10 372 553 24.5 6.3 Table 3 Low temperature toughness of flat-rolled steel plate

[0032] It can be seen that the flatness of the flat-rolled steel plates of Examples 1-2 is less than 3 mm, while the flatness of the flat-rolled steel plate of Comparative Example 1 is 6.3 mm. The flatness of the flat-rolled steel plate of Example 1 is significantly better than that of Comparative Example 1; the -40 degree impact performance of Examples 1-2 is also significantly better than that of Comparative Example 1; by comparison Figure 1 and Figure 2 It can be seen that the microscopic grain size of Example 1 is about 11 μm, the distribution is uniform, and the structure is not coarsened, while the austenite grains of Comparative Example 1 grow abnormally and coarsen, resulting in poor low-temperature toughness of the flat-rolled steel plate of Comparative Example 1. The above analysis results can prove that the technical solution of the present invention can produce a flat-rolled steel plate with high toughness and high flatness.

[0033] Although the present invention has been described in detail by referring to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person skilled in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, and they shall be within the scope of protection of the present invention.

Claims

1. A method for preparing a flat-rolled steel plate with high toughness and high flatness, characterized in that: The chemical composition of the flat-rolled steel plate is C: 0.050%-0.140%, Mn: 0.80%-1.80%, Si≤0.20%, Nb: 0.008%-0.050%, Ti: 0.008%-0.020%, Al≤0.035%, P≤0.015%, S: ≤0.0030%, and the rest is Fe and other unavoidable impurities; At the same time, 0.16%≤(%C)+(%Mn) / 6≤0.19%, 0.045%≤(%Nb)+(%Al)+(%Ti)≤0.070%; The preparation steps of flat-rolled steel plates include: molten iron pretreatment, smelting, refining, continuous casting, billet heating, rolling, cooling, and straightening processes.

2. The method for preparing a flat-rolled steel sheet according to claim 1, characterized in that: The thickness of the flat-rolled steel plate is 6-10mm, the width is >3600mm, and the length is <55m; the yield strength of the flat-rolled steel plate is ≤440MPa, the straightness is ≤3mm / m, and the -40℃ KV2 impact energy is ≥140J.

3. The method for preparing a flat-rolled steel sheet according to claim 1, characterized in that: The smelting process adopts BOF steelmaking process.

4. The method for preparing a flat-rolled steel sheet according to claim 1, characterized in that: The refining process adopts LF refining, and after LF refining, RH vacuum treatment is performed, and then a continuous casting process is performed.

5. The method for preparing a flat-rolled steel sheet according to claim 1, characterized in that: The parameters of the billet heating process are controlled as follows: billet out-of-furnace temperature 1200-1250°C, soaking time 20min≤30min, total heating time / H 1.3min / mm≤1.5min / mm, where H is the billet thickness.

6. The method for preparing a flat-rolled steel sheet according to claim 1, characterized in that: After the ingot is removed from the furnace and descaled by high-pressure water, rolling begins. The rolling is carried out in one stage and completed in the complete recrystallization zone. The first rolling temperature is satisfy: =1027+483×(%C)+896×(%Ti)+373×(%Al)-353×(%Si)+6652×(%Nb)-432×SQRT(%Nb)+862×(%V)-232×SQRT(%V).

7. The method for preparing a flat-rolled steel sheet according to claim 1, characterized in that: The rolling temperature of each of the last 3-4 passes in the rolling process , Export thickness , deformation rate Satisfy 15≤ × / ≤25.

8. The method for preparing a flat-rolled steel sheet according to claim 1, characterized in that: The parameters of the cooling process are controlled as follows: the rolled piece is cooled by water mist after rolling to a temperature of 630-680°C.