Lightweight steel hot-rolled coiled plate and production method thereof
By optimizing chemical composition and process parameters in lightweight steel, high-temperature controlled rolling and differentiated cooling are achieved, the problem of poor hot processing performance of lightweight steel is solved, and the industrial production of hot-rolled coils of lightweight steel is realized and Performance improvement.
Patent Information
- Application Number
- CN202411146577.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing lightweight steel has poor thermal processing performance and is difficult to achieve stable control within a narrow process window, resulting in an increased risk of rolling defects and cracks, limiting the industrial promotion and application of materials.
Through designing chemical components, C: 0.6~1.5%, Si: 0.03~1.0%, Mn: 15~30%, Al: 4.0~10.0%, Ni: ≤5.0%, P: ≤0.020%, S: ≤0.010% , the lightweight steel hot-rolled coil plate with Fe and impurities adopts high-temperature controlled rolling and two cooling process paths to control the rolling pressure and cooling speed to ensure material performance and surface quality.
The industrial production of lightweight steel hot-rolled coils has been realized, which improves the strength and toughness of the material, reduces the rolling load and crack risks, and is suitable for automotive and special engineering machinery applications.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal materials and preparation thereof, and in particular to a light steel hot-rolled coil and a production method thereof. Background Art
[0002] Lightweight steel is made by adding light elements such as C, Al, Si, etc. to steel to reduce the density of the steel. The degree of density reduction depends on the amount of C and Al light elements added. Among them, Al element has the greatest impact on the density of the material. Every 1% addition can reduce the density of the steel by 0.101g / cm 3 . In recent years, it has attracted more and more attention due to its significant weight reduction effect and wide application prospects. According to different phase compositions, lightweight steels are available in ferrite, austenite and duplex types. Among them, ferrite has low strength, duplex is difficult to control hot working, and austenite has excellent forming performance and can take into account both strength and toughness indicators, which has attracted much attention.
[0003] Austenitic lightweight steel generally adds a large amount of austenite stabilizing elements such as Mn to reduce the temperature of austenite to ferrite transformation, so that the hot-rolled steel strip can still retain a large amount of austenite structure at room temperature. However, as the alloy content in the steel increases, the hot processing performance and deformation resistance of the material have changed greatly. How to achieve stable control of the hot rolling process in a narrow process window and avoid the generation of defects is one of the main problems in the current industrial production process, and it is also a difficulty that limits the promotion and application of materials.
[0004] Patent CN111663085A "A hot-rolled austenitic low-density steel with ultra-high strength and plasticity and its production method" adopts smelting and continuous casting into billets; heating the continuous casting; rough rolling; water spray cooling; finishing rolling; rapid heating; coiling; natural cooling to room temperature. This document mainly uses 55-75mm thin billets, and the whole rolling process is controlled at low temperature. The rolling mill load is large, the production difficulty is large, and the risk of rolling cracks increases.
[0005] Patent CN112760568A "A high-strength, high-plasticity, low-density steel and its preparation method" has a production method that includes smelting die-cast steel ingots in a vacuum induction furnace, homogenizing and forging the steel ingots to obtain bars or plates after forging, and then performing solid solution treatment and aging treatment on the bars or plates after forging. The production process and production cycle adopted in this document are relatively long and are not suitable for industrial promotion and application.
[0006] The present invention realizes the industrialized production of light steel hot-rolled coils by implementing the processes of heating, rolling, cooling and the like of light steel ingots with designed components, laying a foundation for further application and promotion of light steel materials in automobiles and special engineering machinery. Summary of the invention
[0007] The purpose of the present invention is to provide a light steel hot-rolled coil and a production method thereof in view of the above problems. The purpose of the present invention is achieved as follows: A light steel hot-rolled coil, the chemical composition and weight percentage content are: C: 0.6~1.5%, Si: 0.03~1.0%, Mn: 15~30%, Al: 4.0~10.0%, Ni: ≤5.0%, P: ≤0.020%, S: ≤0.010%, Nb+V+Ti≤0.25%, the rest is Fe and unavoidable impurities.
[0008] A production method of a light steel hot-rolled coil, comprising the following steps: step one: smelting: continuous casting or die casting into a billet, the billet thickness is controlled at 150-230 mm; step two: rolling: heating the billet, the temperature is controlled at 1180-1270° C., the heating time is 10 mm / 12-20 min; high-pressure water is used to remove scale after leaving the heating furnace; then 1-2 stands are used for rough rolling, the rough rolling passes are 5-7 passes, the single pass reduction rate is ≤15% and the single pass reduction amount is ≤20 mm, the billet outlet temperature at the rough rolling end stand is 1000-1150° C.; the intermediate billet is used for edge heating Heater to ensure the edge temperature is 950~1100℃, and finally use 6~7 stands for finishing rolling, with a single-pass reduction rate of 10~30%, the exit speed of the last stand of finishing rolling is controlled at 3~15m / s, and the final rolling temperature of finishing rolling is controlled at 850~950℃; Step three: Two cooling processes can be used after rolling: Process 1, rapid cooling to ≤350℃ after rolling and then coiling, with a cooling rate of 10~50℃ / s; Process 2, rapid cooling to 600~700℃ after rolling and then coiling, with a cooling rate of 5~20℃ / s, and slow cooling in a holding pit after coiling, with a cooling rate of 5~30℃ / h.
[0009] The beneficial effects of the present invention are: 1. The process method is used to realize the industrialized production of light steel hot-rolled coils.
[0010] 2. The steel has high alloy content, large high-temperature rolling force and poor thermoplasticity. The rolling reduction is controlled in stages during rough rolling and finishing rolling to ensure the surface quality of the coil, and edge heaters are used in the intermediate billet to avoid edge cracks caused by rapid temperature drop at the edge.
[0011] 3. Design two cooling process paths to achieve differentiated control of material properties. DETAILED DESCRIPTION
[0012] The chemical composition design of the lightweight steel in the present invention adopts a fully austenitic structure with a ferrite content of ≤3%. Due to the high alloy content, in order to reduce the rolling load, high-temperature controlled rolling is adopted throughout the process, and two cooling process paths are designed after the steel strip is coiled according to the performance requirements. The design process is as follows: the heating temperature is 1180℃~1270℃, and the holding time is 10mm / 12-20min to ensure that the steel billet is evenly burned and burned through. The rolling reduction rate is controlled in stages during rough rolling and finishing rolling to avoid excessive rolling load or single-pass reduction, thereby causing surface defects. Edge heaters are used for the intermediate billet after rough rolling to ensure the temperature of the edges on both sides and avoid edge cracking during rolling. The final rolling temperature of the steel strip finishing rolling is required to be ≥850℃, and it is directly water-cooled after rolling with a water cooling rate of ≥10℃ / s. The final cooling temperature is ≤350℃, which can avoid the precipitation and growth of κ-phase carbides. In order to improve the strength of the material, the steel strip can also be coiled at a high temperature of 600-700°C and then placed in a slow cooling pit for slow cooling to promote the aging precipitation of κ phase carbides and achieve a secondary improvement in the material strength.
[0013] The components and weight percentage contents of a high-strength light-weight steel hot-rolled coil are as follows: C: 0.6-1.5%, Si: 0.03-1.0%, Mn: 15-30%, Al: 4.0-10.0%, Ni: ≤5.0%, P: ≤0.020%, S: ≤0.010%, Nb+V+Ti≤0.25%, and the rest are Fe and unavoidable impurities.
[0014] A method for producing a high-strength light-weight steel hot-rolled coil, comprising the following steps: (1) smelting and continuously casting or die casting into a billet, wherein the billet thickness is controlled at 150-230 mm; (2) directly heating the billet, wherein the heating temperature is controlled at 1180-1270° C., and the heating time is 10 mm / 12-20 min; (3) descaling the billet by high-pressure water after it leaves the heating furnace; (4) rough rolling is performed by 1-2 stands, wherein the rough rolling passes are 5-7, and the reduction rate of each pass is ≤15%. The reduction of a single pass is ≤20mm, and the outlet temperature of the billet at the rough rolling end stand is 1000-1150℃; (5) The edge heater is used for the intermediate billet to ensure that the edge temperature is 950~1100℃ to avoid edge cracking during rolling; (6) 6~7 stands are used for finishing rolling, the single pass reduction rate is 10-30%, the outlet speed of the finishing end stand is controlled at 3~15m / s, and the finishing temperature is controlled at 850-950℃; (7) After rolling, two cooling processes can be used according to performance requirements. Process 1: After rolling, the steel is quickly cooled to ≤350℃ and then coiled, with a cooling rate of 10-50℃ / s; Process 2: After rolling, the steel is quickly cooled to 600-650℃ and then coiled, with a cooling rate of 5-20℃ / s, and after coiling, it is placed in a heat preservation pit for slow cooling, with a cooling rate of 5-30℃ / h. Example 1
[0015] 1. Smelting: Chemical composition and weight percentage content are: C: 0.8%, Si: 0.20%, Mn: 25%, Al: 6.0%, P: 0.012%, S: 0.003%, Nb: 0.15%. Continuous casting or die casting into billets, the thickness of the billet is 200mm.
[0016] 2. Rolling: (1) Heating of the ingot, heating temperature controlled at 1250℃, heating time 4h; (2) Descaling by high pressure water after leaving the heating furnace; (3) Rough rolling with 1 stand, 7 passes, single pass reduction 10-15mm, intermediate billet thickness 70mm, billet outlet temperature at the final stand of rough rolling 1090℃; (4) Edge heaters are used in the intermediate billet to ensure edge temperature and avoid edge cracking during rolling; (5) Finishing rolling with 7 stands, single pass reduction 3-15mm, final rolling product thickness 10mm, final stand exit speed controlled at 4.5m / s, final rolling temperature 930℃; (6) Rapid cooling to 280℃ after rolling, coiling, cooling rate 15℃ / s. (7) The yield strength of the material is 867MPa, the tensile strength is 1060MPa, and the elongation after fracture is 48%. Example 2
[0017] 1. Smelting: Chemical composition and weight percentage content are: C: 1.2%, Si: 0.15%, Mn: 29%, Al: 9.6%, P: 0.010%, S: 0.004%, Ni: 1.5%, V: 0.2%. Continuous casting or die casting into billets, the thickness of the billet is 150mm.
[0018] 2. Rolling: (1) Heating of the ingot, heating temperature controlled at 1230℃, heating time 4h; (2) After leaving the heating furnace, high-pressure water is used for descaling once; (3) Rough rolling is performed using 1 stand, 7 passes are performed, the reduction per pass is 10-15mm, the thickness of the intermediate billet is 50mm, and the outlet temperature of the billet at the final stand of rough rolling is 1050℃; (4) Edge heaters are used for the intermediate billet to ensure the edge temperature and avoid edge cracking during rolling; (5) Finishing rolling is performed using 7 stands, the reduction per pass is 3-15mm, the thickness of the final rolled product is 5mm, the outlet speed of the final stand of the finishing rolling is controlled at 6m / s, and the final rolling temperature of the finishing rolling is 890℃; (6) After rolling, the steel strip is rapidly cooled to 650℃ at a cooling rate of 15℃ / s and coiled. After coiling, the steel strip is directly placed in a slow cooling pit for insulation at a cooling rate of about 25℃ / h. After two days, it is hoisted out for performance inspection. (7) The material yield strength is 960 MPa, the tensile strength is 1230 MPa, and the elongation after fracture is 32%.
[0019] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.
Claims
1. A lightweight hot-rolled steel coil, Features: The chemical composition and weight percentage content are: C: 0.6~1.5%, Si: 0.03~1.0%, Mn: 15~30%, Al: 4.0~10.0%, Ni: ≤5.0%, P: ≤0.020%, S: ≤0.010%, Nb+V+Ti≤0.25%, and the rest are Fe and unavoidable impurities.
2. A method for producing a light steel hot-rolled coil, Features: The following steps are involved: Step 1: Smelting: continuous casting or die casting into billets, the thickness of the billets is controlled at 150~230mm; Step 2: rolling: heating the ingot, the temperature is controlled at 1180~1270℃, the heating time is 10mm / 12~20min; high-pressure water is used for descaling after leaving the heating furnace; then 1~2 stands are used for rough rolling, the rough rolling passes are 5~7 passes, the single pass reduction rate is ≤15% and the single pass reduction amount is ≤20mm, and the outlet temperature of the billet at the rough rolling end stand is 1000~1150℃; the edge heater is used for the intermediate billet to ensure that the edge temperature is 950~1100℃, and finally 6~7 stands are used for finishing rolling, the single pass reduction rate is 10~30%, the outlet speed of the finishing rolling end stand is controlled at 3~15m / s, and the finishing rolling temperature is controlled at 850~950℃; Step 3: Two cooling processes can be used after rolling: process one, after rolling, quickly cool to ≤350℃ and then coil it, with a cooling rate of 10~50℃ / s; process two, after rolling, quickly cool to 600~700℃ and then coil it, with a cooling rate of 5~20℃ / s, and after coiling, put it into the insulation pit for slow cooling, with a cooling rate of 5~30℃ / h.
Citation Information
Patent Citations
Manufacturing method of low-density, high-strength and high-toughness hot-rolled steel plate
CN114657441A
Method for producing low-density, high-strength and high-toughness protective steel plate from continuous casting sheet billet
CN116926404A
Nb, V and Ti alloyed light wear-resistant steel as well as preparation method and application thereof
CN117418171A
Rolling method of 2500mm ultra-wide low-density high-strength high-toughness hot-rolled steel plate
CN118122771A
Smelting method of Fe-Mn-Al-C austenitic low-density steel
CN118345298A
Cited By
An austenitic light weight steel hot rolled steel strip and method of manufacture
CN123043423A