Preparation method of intermediate layer for target welding

By adopting the dual fixation form of bonding fixation and magnetic adsorption strengthening in semiconductor target welding, the problems of deformation and offset of intermediate media during processing are solved, and the pass rate and processing quality of target welding are improved.

CN119040816AActive Publication Date: 2024-11-29KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411138494.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-29
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

During the production process of semiconductor targets, intermediate media is prone to deformation or offset during processing, resulting in welding failure. The existing clamping and fixing methods cause damage to the surface of the media, making it difficult to meet product requirements.

Method used

The double fixing form of bonding fixing and magnetic adsorption strengthening is adopted. By laying a pressing layer on the work surface and setting up a strong magnetic component, the stability of the intermediate workpiece during the processing process is ensured and deformation and deviation are avoided.

Benefits of technology

It improves the processing effect of the intermediate layer, reduces the defect rate of workpieces, significantly improves the pass rate of target welding, and simplifies process operations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040816A_ABST
    Figure CN119040816A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a middle layer for target welding. The preparation method comprises the following steps: (1) laying a first caulking layer on a working table; (2) a middle workpiece is provided, a second adhesive pressing layer is arranged on the surface of the middle workpiece, and the side, provided with the second adhesive pressing layer, of the middle workpiece is attached to the first adhesive pressing layer, so that the middle workpiece is fixedly attached to the working table; (3) a strong magnetic assembly is provided, and the middle workpiece is fixed in a reinforced mode through the strong magnetic assembly; fourthly, the intermediate workpiece is subjected to primary machining treatment, and an intermediate blank is obtained; and (V) taking down the intermediate material blank, overturning, repeating the steps (II) and (III), and carrying out secondary processing treatment on the intermediate material blank to obtain the intermediate layer. The problem that the middle workpiece deforms or deviates in the machining process is solved, and therefore the reject ratio of the workpiece is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor target material production and relates to a method for preparing an intermediate layer for target material welding. Background Art

[0002] In the production process of semiconductor targets, dissimilar metal welding technology plays an important role. Hot isostatic pressing diffusion welding is a relatively efficient and widely used dissimilar metal welding method. In order to ensure the effectiveness of welding, an intermediate medium compatible with the metal (target substrate) and the metal (back plate) of special materials is added, so that the three metal molecules diffuse with each other under specific conditions, thereby achieving the purpose of welding two different metals together. Due to the particularity of diffusion welding, the commonly used intermediate medium has the characteristics of thin thickness, large diameter and soft material, which increases the difficulty of machining the intermediate medium.

[0003] After welding, the target material needs to test the welding bonding rate of the back plate and the target material substrate. The size and quality of the intermediate medium are very important for the welding bonding rate. If the intermediate medium has a size deviation, it is easy to cause welding failure and target failure. During the manufacturing process, due to the particularity of its material and process requirements, the intermediate medium is usually fixed with a clamping tool before machining. However, the existing clamping and fixing method is prone to damage the surface of the intermediate medium, causing it to deform, and as the machining is carried out, the intermediate medium moves, causing its appearance size to deviate, which cannot meet product requirements.

[0004] Therefore, improving the fixing method during the processing of the intermediate medium is very important for improving the quality of the manufactured products. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing an intermediate layer for target welding, which solves the problem that the workpiece is easily deformed or offset during the processing, thereby causing the workpiece to be unqualified.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for preparing an intermediate layer for target welding, the preparation method comprising:

[0008] (I) Laying the first glue layer on the work surface;

[0009] (II) providing an intermediate workpiece, disposing a second adhesive layer on the surface of the intermediate workpiece, and placing the intermediate workpiece on the first adhesive layer from the side where the second adhesive layer is disposed, so that the intermediate workpiece is adhered and fixed on the work surface;

[0010] (III) providing a strong magnetic component to strengthen the fixation of the intermediate workpiece by using the strong magnetic component;

[0011] (IV) subsequently processing the intermediate workpiece once to obtain an intermediate blank;

[0012] (V) removing the intermediate blank and turning it over, repeating steps (II) and (III), and performing secondary processing on the intermediate blank to obtain an intermediate layer.

[0013] It should be noted that, after one processing, the present invention only completes the processing of one side surface of the intermediate workpiece. When processing the other side surface, it is necessary to first remove the strong magnetic component, then take down the intermediate blank, and remove the original second glue layer. Then, turn the intermediate blank over, repeat steps (II) and (III) to re-set the second glue layer on the other side surface, and after strengthening and fixing it with the strong magnetic component, perform secondary processing on the other side surface.

[0014] As a preferred technical solution of the present invention, the area of ​​the first adhesive layer is greater than the area of ​​the second adhesive layer.

[0015] The first adhesive layer is formed by a plurality of first strip-shaped adhesive tapes arranged at intervals.

[0016] In the present invention, the first glue layer should completely cover the second glue layer to avoid the intermediate workpiece from shifting.

[0017] As a preferred technical solution of the present invention, the second glue layer is formed by a plurality of second strip-shaped adhesive tapes arranged at intervals, and both ends of the second strip-shaped adhesive tapes extend out of the intermediate workpiece respectively.

[0018] Preferably, the second strip tape comprises a first adhesive portion, a connecting portion and a second adhesive portion which are arranged side by side in sequence, the first adhesive portion and the second adhesive portion are independently single-sided adhesives, the connecting portion is a double-sided adhesive, and the connecting portion is used to connect the first adhesive layer.

[0019] In the present invention, the first bonding part and the second bonding part are bonded and fixed on the intermediate workpiece, one side of the connecting part is bonded to the intermediate workpiece, and the other side is bonded to the first glue layer on the worktable, thereby achieving preliminary fixation of the intermediate workpiece.

[0020] Preferably, the width of the second strip-shaped tape is smaller than the width of the first strip-shaped tape.

[0021] Preferably, after the intermediate workpiece is attached to the first adhesive layer, the first strip-shaped adhesive tape of the first adhesive layer and the second strip-shaped adhesive tape of the second adhesive layer are arranged at an angle.

[0022] Preferably, the first strip-shaped adhesive tape of the first adhesive layer and the second strip-shaped adhesive tape of the second adhesive layer are arranged perpendicularly.

[0023] As a preferred technical solution of the present invention, the strong magnetic component includes at least one magnet and a third laminated adhesive layer covering the magnet.

[0024] Preferably, a hanging ring is also provided on the magnet.

[0025] Preferably, the enhanced fixation comprises: placing the strong magnetic component on the surface of the intermediate workpiece so that the intermediate workpiece is adsorbed on the work surface.

[0026] As a preferred technical solution of the present invention, the preparation method further comprises: before providing the first adhesive layer, performing a first cleaning treatment on the work surface.

[0027] Preferably, the first cleaning process comprises: wiping the work surface with a cleaning agent to remove oil stains on the work surface.

[0028] Preferably, the cleaning agent comprises isopropanol and / or ethanol.

[0029] As a preferred technical solution of the present invention, the preparation method further comprises: before providing the second adhesive layer, performing a second cleaning treatment on the intermediate workpiece or the intermediate blank.

[0030] Preferably, the second cleaning process comprises: ultrasonic cleaning using an organic solvent and pure water in sequence, followed by drying.

[0031] Preferably, the organic solvent includes any one of isopropanol, ethanol or kerosene, or a combination of at least two of them.

[0032] Preferably, the ultrasonic cleaning time is 120 to 240 s, for example, it can be 120 s, 130 s, 140 s, 150 s, 160 s, 170 s, 180 s, 190 s, 200 s, 210 s, 220 s, 230 s or 240 s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the temperature of the ultrasonic cleaning is 20-30°C, for example, it can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] As a preferred technical solution of the present invention, the preparation method further comprises: performing a third cleaning treatment on the magnet before coating the third glue layer.

[0035] Preferably, the third cleaning process comprises: wiping the outer surface of the magnet with a cleaning agent to remove oil stains on the surface of the magnet.

[0036] Preferably, the cleaning agent comprises isopropanol and / or ethanol.

[0037] The present invention cleans the work surface, the intermediate workpiece and the strong magnetic component respectively to remove surface dirt, which is beneficial to improving the firmness between the work surface and the intermediate workpiece, effectively preventing the intermediate workpiece from moving, and ensuring the processing quality.

[0038] As a preferred technical solution of the present invention, the preparation method further includes: before the primary processing or the secondary processing, knocking the surface of the intermediate workpiece or the intermediate blank so that the intermediate workpiece or the intermediate blank is completely fitted with the work surface.

[0039] As a preferred technical solution of the present invention, the one-time processing includes: cutting and polishing the intermediate workpiece in sequence.

[0040] The present invention performs cutting processing on the intermediate workpiece to obtain the shape and size of the intermediate blank that can adapt to the target material welding, and performs polishing processing to remove the concavo-convex or defects on the surface of the intermediate blank to ensure the surface flatness.

[0041] Preferably, the secondary processing comprises: polishing the intermediate blank.

[0042] Preferably, the middle layer is circular or rectangular.

[0043] Preferably, the thickness of the middle layer is 2.2-2.35 mm, for example, it can be 2.2 mm, 2.21 mm, 2.22 mm, 2.23 mm, 2.24 mm, 2.25 mm, 2.26 mm, 2.28 mm, 2.3 mm, 2.31 mm, 2.32 mm, 2.33 mm, 2.34 mm or 2.35 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the roughness of the intermediate layer is ≤1.6 μm.

[0045] Preferably, the planarity of the intermediate layer is ≤0.1 mm.

[0046] Preferably, after the secondary processing is completed, the strong magnetic component is removed, and the first adhesive layer, the second adhesive layer and the third adhesive layer are scraped off.

[0047] As a preferred technical solution of the present invention, the intermediate workpiece is made of aluminum and / or titanium.

[0048] Preferably, the purity of the intermediate workpiece is ≥ 99.6%.

[0049] Exemplarily, the method for preparing the intermediate layer for target welding provided by the present invention specifically comprises the following steps:

[0050] (1) performing a first cleaning process on the work surface, and then laying a first glue layer on the work surface;

[0051] (2) providing an intermediate workpiece, wherein the intermediate workpiece has a first surface and a second surface opposite to each other;

[0052] (3) performing a second cleaning process on the intermediate workpiece, then providing a second adhesive layer on the first surface of the intermediate workpiece, and placing the intermediate workpiece on the first adhesive layer from the side provided with the second adhesive layer, so that the intermediate workpiece is adhered and fixed on the work surface;

[0053] (4) providing at least one magnet, performing a third cleaning treatment on the magnet, and then coating the outer surface of the magnet with a third adhesive layer to obtain a strong magnetic component, placing the strong magnetic component on the second surface of the intermediate workpiece so that the intermediate workpiece is adsorbed on the work surface, and knocking the intermediate workpiece from one side of the second surface so that the intermediate workpiece is completely attached to the work surface;

[0054] (5) Then, the second surface of the intermediate workpiece on the work surface is processed once to obtain an intermediate blank;

[0055] (6) After removing the intermediate blank, turn it over and repeat steps (3) and (4), fix the second surface of the intermediate blank on the work surface, and perform secondary processing on the first surface to obtain an intermediate layer.

[0056] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] The present invention provides a method for preparing an intermediate layer for target material welding. By improving the fixing method of the intermediate workpiece, a dual fixing method of adhesive fixing and magnetic adsorption strengthening is adopted to avoid deformation or displacement of the workpiece during processing, thereby improving the processing effect, reducing the defective rate of the workpiece, and greatly improving the welding qualification rate of the target material. The process is simple and the operation is convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 It is a schematic diagram of fixing the intermediate workpiece on the work surface according to Embodiment 1 of the present invention;

[0060] Figure 2 This is a schematic diagram of an intermediate blank fixed on a work surface according to Example 1 of the present invention;

[0061] Figure 3 This is a schematic diagram of the intermediate workpiece of Comparative Example 1 of the present invention being fixed on a work surface;

[0062] Figure 4 This is a schematic diagram of the intermediate blank of Comparative Example 1 of the present invention being fixed on a work surface;

[0063] Figure 5 This is a schematic diagram of the intermediate workpiece of Comparative Example 2 of the present invention being fixed on a work surface;

[0064] Figure 6 This is a schematic diagram of the intermediate blank of Comparative Example 2 of the present invention being fixed on a work surface.

[0065] Among them, 1-working table; 101-first glue pressing layer; 2-intermediate workpiece; 201-second glue pressing layer; 2011-first bonding part; 2012-connecting part; 2013-second bonding part; 3-intermediate blank; 4-strong magnetic component; 401-third glue pressing layer; 5-support table; 6-pressing plate. DETAILED DESCRIPTION

[0066] It should be understood that, in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.

[0067] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0068] In a specific embodiment, the present invention provides a method for preparing an intermediate layer for target welding, the preparation method comprising:

[0069] (I) Laying the first glue layer on the work surface;

[0070] (II) providing an intermediate workpiece, disposing a second adhesive layer on the surface of the intermediate workpiece, and placing the intermediate workpiece on the first adhesive layer from the side where the second adhesive layer is disposed, so that the intermediate workpiece is adhered and fixed on the work surface;

[0071] (III) providing a strong magnetic component to strengthen the fixation of the intermediate workpiece by using the strong magnetic component;

[0072] (IV) subsequently processing the intermediate workpiece once to obtain an intermediate blank;

[0073] (V) removing the intermediate blank and turning it over, repeating steps (II) and (III), and performing secondary processing on the intermediate blank to obtain an intermediate layer.

[0074] In step (I), the preparation method further comprises: before providing the first adhesive layer, performing a first cleaning treatment on the work surface. Specifically, the first cleaning treatment comprises: wiping the work surface with a cleaning agent to remove oil stains on the work surface. The cleaning agent comprises isopropyl alcohol and / or ethanol.

[0075] The area of ​​the first adhesive layer is larger than that of the second adhesive layer, so as to completely cover the second adhesive layer.

[0076] Specifically, the first adhesive layer is formed by a plurality of first strip-shaped adhesive tapes arranged at intervals.

[0077] In step (II), the intermediate workpiece is made of aluminum and / or titanium, and the purity of the intermediate workpiece is ≥99.6%. Preferably, the intermediate workpiece is made of aluminum, specifically A1060.

[0078] In some embodiments, the second adhesive layer is formed by a plurality of second strip-shaped adhesive tapes disposed at intervals, and two ends of the second strip-shaped adhesive tapes extend out of the intermediate workpiece respectively.

[0079] Furthermore, the second strip-shaped adhesive tape comprises a first adhesive portion, a connecting portion and a second adhesive portion arranged side by side in sequence, the first adhesive portion and the second adhesive portion are independently single-sided adhesive, the connecting portion is double-sided adhesive, and the connecting portion is used to connect the first adhesive layer. The first adhesive portion and the second adhesive portion are bonded and fixed to the intermediate workpiece, one side of the connecting portion is bonded to the intermediate workpiece, and the other side of the connecting portion is bonded to the first adhesive layer on the worktable, thereby achieving preliminary fixation of the intermediate workpiece.

[0080] Specifically, the width of the second strip-shaped tape is smaller than the width of the first strip-shaped tape.

[0081] In some embodiments, after the intermediate workpiece is attached to the first adhesive layer, the first strip of adhesive tape of the first adhesive layer and the second strip of adhesive tape of the second adhesive layer are arranged at an angle. Preferably, the first strip of adhesive tape of the first adhesive layer and the second strip of adhesive tape of the second adhesive layer are arranged perpendicularly.

[0082] In some embodiments, the preparation method further comprises: before setting the second adhesive layer, performing a second cleaning treatment on the intermediate workpiece or intermediate blank. Specifically, the second cleaning treatment comprises: ultrasonic cleaning with organic solvent and pure water in sequence, and then drying. The organic solvent comprises any one of isopropanol, ethanol or kerosene or a combination of at least two. The ultrasonic cleaning time is 120 to 240 seconds, and the ultrasonic cleaning temperature is 20 to 30°C.

[0083] In step (III), the strong magnetic assembly includes at least one magnet and a third glue layer covering the magnet. Specifically, a hanging ring is provided on the magnet to facilitate the staff to take and operate.

[0084] The enhanced fixation includes: placing the strong magnetic component on the second surface of the intermediate workpiece so that the intermediate workpiece is adsorbed on the work surface.

[0085] In some embodiments, the preparation method further comprises: performing a third cleaning treatment on the magnet before coating the third adhesive layer. Specifically, the third cleaning treatment comprises: wiping the outer surface of the magnet with a cleaning agent to remove oil stains on the surface of the magnet. The cleaning agent comprises isopropyl alcohol and / or ethanol.

[0086] In step (IV), the primary processing includes: cutting and polishing the intermediate workpiece in sequence.

[0087] In step (V), the secondary processing includes: polishing the intermediate blank.

[0088] In step (IV) or (V), the preparation method further comprises: before the primary processing or the secondary processing, striking the intermediate workpiece or the intermediate blank so that the intermediate workpiece or the intermediate blank is completely fitted with the work surface.

[0089] In some embodiments, the middle layer is circular or rectangular, the thickness of the middle layer is 2.2-2.35 mm, the roughness of the middle layer is ≤1.6 μm, and the flatness of the middle layer is ≤0.1 mm.

[0090] In some embodiments, after the secondary processing is completed, the strong magnetic component is removed, and the first adhesive layer, the second adhesive layer and the third adhesive layer are scraped off.

[0091] In another specific embodiment, the present invention provides a method for target welding using an intermediate layer prepared by the preparation method described in a specific embodiment, which specifically comprises the following steps:

[0092] S1: providing a target material, an intermediate layer and a back plate, respectively setting threads on the welding surfaces of the target material and the back plate, and pressing the threads on the welding surface of the target material into the intermediate layer, and then performing heat treatment to obtain an intermediate welding material;

[0093] S2: applying pressure to the intermediate welding material in step S1, so that the back plate and the intermediate welding material are assembled to obtain a target assembly;

[0094] S3: placing the target assembly of step S2 in a package for hot isostatic pressing welding.

[0095] Example 1

[0096] This embodiment provides a method for preparing an intermediate layer for target welding, which specifically includes the following steps:

[0097] (1) Wiping the work surface with ethanol to remove oil stains on the work surface, and then laying a first adhesive layer on the work surface, the first adhesive layer being formed by three first strips of adhesive tapes arranged at intervals, and each first strip of adhesive tape having a width of 220 mm;

[0098] (2) providing an aluminum intermediate workpiece having a first surface and a second surface opposite to each other;

[0099] (3) At 25° C., the intermediate workpiece is first ultrasonically cleaned with isopropyl alcohol for 180 seconds, then ultrasonically cleaned with pure water for 150 seconds, and then dried. A second adhesive layer is then provided on the first surface of the intermediate workpiece, such as Figure 1 As shown, the first surface of the intermediate workpiece is pasted on the first adhesive layer, so that the intermediate workpiece is pasted and fixed on the worktable, the second adhesive layer is formed by six second strip-shaped adhesive tapes arranged at intervals, and the two ends of the second strip-shaped adhesive tapes extend out of the intermediate workpiece to completely cover the intermediate workpiece, the width of the second strip-shaped adhesive tape is 40 mm, and the second strip-shaped adhesive tape includes a first adhesive portion, a connecting portion and a second adhesive portion arranged side by side in sequence, the first adhesive portion and the second adhesive portion are independently single-sided adhesive, and the connecting portion is double-sided adhesive;

[0100] (4) providing two magnets, wiping the outer surfaces of the magnets with ethanol to remove oil stains on the surfaces of the magnets, and then coating the outer surfaces of the magnets with a third glue layer to obtain a strong magnetic assembly, placing the strong magnetic assembly on the second surface of the intermediate workpiece so that the intermediate workpiece is adsorbed on the work surface, knocking the intermediate workpiece from one side of the second surface so that the intermediate workpiece and the work surface are completely attached, and then cutting and polishing the intermediate workpiece on the work surface in sequence;

[0101] (5) After removing the strong magnetic component, take out the intermediate blank, scrape off the second glue layer on the first surface, and repeat step (3). Figure 2 As shown, a second adhesive layer is arranged on the second surface, and the second surface of the intermediate blank is pasted on the first adhesive layer, so that the intermediate blank is pasted and fixed on the work surface, the second adhesive layer is formed by six second strip-shaped adhesive tapes arranged at intervals, and the two ends of the second strip-shaped adhesive tapes extend out of the intermediate workpiece to completely cover the intermediate workpiece, the width of the second strip-shaped adhesive tape is 40 mm, and the second strip-shaped adhesive tape includes a first adhesive portion, a connecting portion and a second adhesive portion arranged side by side in sequence, the first adhesive portion and the second adhesive portion are independently single-sided adhesive, and the connecting portion is double-sided adhesive;

[0102] (6) placing the strong magnetic component in step (4) on the first surface of the intermediate blank so that the intermediate workpiece is adsorbed on the work surface, then striking the intermediate blank from one side of the first surface so that the intermediate blank is completely attached to the work surface, and then polishing the first surface to obtain an intermediate layer;

[0103] (7) Remove the strong magnetic component and scrape off the first, second and third adhesive layers.

[0104] Example 2

[0105] This embodiment provides a method for preparing an intermediate layer for target welding, which specifically includes the following steps:

[0106] (1) Wiping the work surface with ethanol to remove oil stains on the work surface, and then laying a first adhesive layer on the work surface, the first adhesive layer being formed by four first strips of adhesive tapes arranged at intervals, and each first strip of adhesive tape having a width of 150 mm;

[0107] (2) providing a titanium intermediate workpiece having a first surface and a second surface opposite to each other;

[0108] (3) At 30° C., the intermediate workpiece is first ultrasonically cleaned with ethanol for 60 seconds, then ultrasonically cleaned with pure water for 100 seconds, and then dried. Subsequently, a second adhesive layer is provided on the first surface of the intermediate workpiece, and the first surface of the intermediate workpiece is attached to the first adhesive layer, so that the intermediate workpiece is adhered and fixed on the work surface, the second adhesive layer is formed by seven second strips of adhesive tape arranged at intervals, and the two ends of the second strips of adhesive tape extend out of the intermediate workpiece to completely cover the intermediate workpiece, the width of the second strip of adhesive tape is 40 mm, and the second strip of adhesive tape includes a first adhesive portion, a connecting portion, and a second adhesive portion arranged side by side in sequence, the first adhesive portion and the second adhesive portion are independently single-sided adhesive, and the connecting portion is double-sided adhesive;

[0109] (4) providing two magnets, wiping the outer surfaces of the magnets with ethanol to remove oil stains on the surfaces of the magnets, and then coating the outer surfaces of the magnets with a third glue layer to obtain a strong magnetic assembly, placing the strong magnetic assembly on the second surface of the intermediate workpiece so that the intermediate workpiece is adsorbed on the work surface, knocking the intermediate workpiece from one side of the second surface so that the intermediate workpiece and the work surface are completely attached, and then cutting and polishing the intermediate workpiece on the work surface in sequence;

[0110] (5) After removing the strong magnetic component, take out the intermediate blank, scrape off the second glue layer on the first surface, repeat step (3) to set the second glue layer on the second surface, and stick the second surface of the intermediate blank on the first glue layer, so that the intermediate blank is glued and fixed on the work surface, the second glue layer is formed by seven second strips of tape arranged at intervals, and the two ends of the second strips of tape extend out of the intermediate workpiece to completely cover the workpiece, the width of the second strip of tape is 40 mm, and the second strip of tape includes a first adhesive portion, a connecting portion and a second adhesive portion arranged side by side in sequence, the first adhesive portion and the second adhesive portion are independently single-sided adhesive, and the connecting portion is double-sided adhesive;

[0111] (6) placing the strong magnetic component of step (4) on the first surface of the intermediate blank so that the intermediate workpiece is adsorbed on the work surface, then striking the intermediate blank from one side of the first surface so that the intermediate blank is completely attached to the work surface, and then polishing the first surface to obtain an intermediate layer;

[0112] (7) Remove the strong magnetic component and scrape off the first, second and third adhesive layers.

[0113] Example 3

[0114] This embodiment provides a method for preparing an intermediate layer for target welding, which specifically includes the following steps:

[0115] (1) Wiping the work surface with isopropyl alcohol to remove oil stains on the work surface, and then laying a first adhesive layer on the work surface, the first adhesive layer being formed by four first strips of adhesive tapes arranged at intervals, and each first strip of adhesive tape having a width of 160 mm;

[0116] (2) providing an aluminum intermediate workpiece having a first surface and a second surface opposite to each other;

[0117] (3) At 20° C., the intermediate workpiece is first ultrasonically cleaned with ethanol for 180 seconds, then ultrasonically cleaned with pure water for 180 seconds, and then dried. Subsequently, a second adhesive layer is provided on the first surface of the intermediate workpiece, and the first surface of the intermediate workpiece is attached to the first adhesive layer, so that the intermediate workpiece is adhered and fixed on the work surface, the second adhesive layer is formed by seven second strips of adhesive tape arranged at intervals, and the two ends of the second strips of adhesive tape extend out of the intermediate workpiece to completely cover the intermediate workpiece, the width of the second strip of adhesive tape is 30 mm, and the second strip of adhesive tape includes a first adhesive portion, a connecting portion and a second adhesive portion arranged side by side in sequence, the first adhesive portion and the second adhesive portion are independently single-sided adhesive, and the connecting portion is double-sided adhesive;

[0118] (4) providing two magnets, wiping the outer surfaces of the magnets with ethanol to remove oil stains on the surfaces of the magnets, and then coating the outer surfaces of the magnets with a third glue layer to obtain a strong magnetic assembly, placing the strong magnetic assembly on the second surface of the intermediate workpiece so that the intermediate workpiece is adsorbed on the work surface, knocking the intermediate workpiece from one side of the second surface so that the intermediate workpiece and the work surface are completely attached, and then cutting and polishing the intermediate workpiece on the work surface in sequence;

[0119] (5) After removing the strong magnetic component, take out the intermediate blank, scrape off the second glue layer on the first surface, repeat step (3) to set the second glue layer on the second surface, and stick the second surface of the intermediate blank on the first glue layer, so that the intermediate blank is glued and fixed on the work surface, the second glue layer is formed by seven second strips of tape arranged at intervals, and the two ends of the second strips of tape extend out of the intermediate workpiece to completely cover the workpiece, the width of the second strip of tape is 30 mm, and the second strip of tape includes a first adhesive portion, a connecting portion and a second adhesive portion arranged side by side in sequence, the first adhesive portion and the second adhesive portion are independently single-sided adhesive, and the connecting portion is double-sided adhesive;

[0120] (6) placing the strong magnetic component of step (4) on the first surface of the intermediate blank so that the intermediate workpiece is adsorbed on the work surface, then striking the intermediate blank from one side of the first surface so that the intermediate blank is completely attached to the work surface, and then polishing the first surface to obtain an intermediate layer;

[0121] (7) Remove the strong magnetic component and scrape off the first, second and third adhesive layers.

[0122] Comparative Example 1

[0123] This comparative example provides a method for preparing an intermediate layer for target welding, which is different from Example 1 in that: Figure 3 and Figure 4 As shown, no strong magnetic component is used to strengthen and fix the intermediate workpiece, and the remaining preparation steps and process parameters are the same as those in Example 1.

[0124] Comparative Example 2

[0125] This comparative example provides a method for preparing an intermediate layer for target welding, which specifically comprises the following steps:

[0126] (1) providing an aluminum intermediate workpiece having a first surface and a second surface opposite to each other;

[0127] (2) Provide universal fixtures, such as Figure 5 As shown, the universal fixture includes a support table, on which two pressing plates are movably arranged, and the two pressing plates are symmetrically arranged;

[0128] (3) Wipe the work surface with isopropyl alcohol to remove the oil stains on the work surface, and then fix the universal fixture on the work surface;

[0129] (4) at 20° C., the intermediate workpiece is firstly ultrasonically cleaned with ethanol for 180 seconds, then ultrasonically cleaned with pure water for 150 seconds, and then dried, and then a glue layer is provided on the first surface of the intermediate workpiece, wherein the glue layer is formed by five strips of adhesive tapes arranged at intervals;

[0130] (5) placing the first surface of the intermediate workpiece on the support table, clamping and fixing the intermediate workpiece with a pressing plate, and then cutting and polishing the intermediate workpiece on the worktable in sequence to obtain an intermediate blank;

[0131] (6) Remove the intermediate blank and repeat step (4) to provide a glue layer on the second surface of the intermediate workpiece. Figure 6 As shown, the second surface of the intermediate blank is placed on the support table, the intermediate blank is clamped and fixed by a pressing plate, and then the first surface of the intermediate blank is polished to obtain an intermediate layer.

[0132] The present invention uses the intermediate layer prepared by the preparation method provided in Examples 1 to 3 and Comparative Examples 1 and 2 to perform target welding, and tests the target welding qualification rate. The results are shown in Table 1.

[0133] Target welding specifically includes the following steps:

[0134] S1: providing a target material, an intermediate layer and a back plate, respectively setting threads on the welding surfaces of the target material and the back plate, and pressing the threads on the welding surface of the target material into the intermediate layer, and then heat treating the target material and the intermediate layer to obtain an intermediate welding material;

[0135] S2: applying pressure to the intermediate welding material in step S1, so that the back plate and the intermediate welding material are assembled to obtain a target assembly;

[0136] S3: placing the target assembly of step S2 in a package for hot isostatic pressing welding.

[0137] Table 1

[0138] serial number Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 thickness 2.3mm 2.26mm 2.31mm 2.3mm 2.3mm Roughness 1.5μm 1.6μm 1.5μm 2.3μm 2.1μm Flatness ≤0.1mm ≤0.1mm ≤0.1mm ≤0.8mm ≤1.2mm Welding pass rate 100% 100% 100% 97.3% 97%

[0139] It is not difficult to see from Table 1 that the roughness of the intermediate layer prepared by Examples 1 to 3 is low and the surface is flat, and a higher target welding rate is obtained. Compared with Example 1, in the preparation process of the intermediate layer, Comparative Example 1 did not use a strong magnetic component for enhanced fixation, resulting in the workpiece being offset during the machining process, reducing the flatness of the intermediate layer, and further affecting the welding pass rate of the target and the back plate. Compared with Examples 1 to 3, Comparative Example 2 uses a universal clamp to clamp and fix the intermediate workpiece, causing a slight deformation of the intermediate workpiece, reducing the quality of the intermediate layer, and reducing the welding pass rate of the target and the back plate.

[0140] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing an intermediate layer for target welding, characterized in that: The preparation method comprises: (I) Laying the first glue layer on the work surface; (II) providing an intermediate workpiece, disposing a second adhesive layer on the surface of the intermediate workpiece, and placing the intermediate workpiece on the first adhesive layer from the side where the second adhesive layer is disposed, so that the intermediate workpiece is adhered and fixed on the work surface; (III) providing a strong magnetic component to strengthen the fixation of the intermediate workpiece by using the strong magnetic component; (IV) subsequently processing the intermediate workpiece once to obtain an intermediate blank; (V) removing the intermediate blank and turning it over, repeating steps (II) and (III), and performing secondary processing on the intermediate blank to obtain an intermediate layer.

2. The preparation method according to claim 1, characterized in that: The area of ​​the first adhesive layer is greater than the area of ​​the second adhesive layer; The first adhesive layer is formed by a plurality of first strip-shaped adhesive tapes arranged at intervals.

3. The preparation method according to claim 2, characterized in that: The second adhesive layer is formed by a plurality of second strip-shaped adhesive tapes arranged at intervals, and two ends of the second strip-shaped adhesive tapes extend out of the intermediate workpiece respectively; Preferably, the second strip-shaped adhesive tape comprises a first adhesive portion, a connecting portion and a second adhesive portion which are sequentially arranged side by side, the first adhesive portion and the second adhesive portion are independently single-sided adhesives, the connecting portion is a double-sided adhesive, and the connecting portion is used to connect the first adhesive layer; Preferably, the width of the second strip of tape is smaller than the width of the first strip of tape; Preferably, after the intermediate workpiece is attached to the first adhesive layer, the first strip of adhesive tape of the first adhesive layer and the second strip of adhesive tape of the second adhesive layer are arranged at an angle; Preferably, the first strip-shaped adhesive tape of the first adhesive layer and the second strip-shaped adhesive tape of the second adhesive layer are arranged perpendicularly.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The strong magnetic component includes at least one magnet and a third glue layer covering the magnet; Preferably, a hanging ring is also provided on the magnet; Preferably, the enhanced fixation comprises: placing the strong magnetic component on the surface of the intermediate workpiece so that the intermediate workpiece is adsorbed on the work surface.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The preparation method further comprises: before providing the first adhesive layer, performing a first cleaning process on the work surface; Preferably, the first cleaning process includes: wiping the work surface with a cleaning agent to remove oil stains on the work surface; Preferably, the cleaning agent comprises isopropanol and / or ethanol.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The preparation method further comprises: before providing the second adhesive layer, performing a second cleaning process on the intermediate workpiece or the intermediate blank; Preferably, the second cleaning process comprises: ultrasonic cleaning using an organic solvent and pure water in sequence, followed by drying; Preferably, the organic solvent comprises any one of isopropanol, ethanol or kerosene or a combination of at least two thereof; Preferably, the ultrasonic cleaning time is 120 to 240 seconds; Preferably, the temperature of the ultrasonic cleaning is 20-30°C.

7. The preparation method according to claim 4, characterized in that: The preparation method further comprises: performing a third cleaning process on the magnet before coating the third adhesive layer; Preferably, the third cleaning process comprises: wiping the outer surface of the magnet with a cleaning agent to remove oil stains on the surface of the magnet; Preferably, the cleaning agent comprises isopropanol and / or ethanol.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method further comprises: before the primary processing or the secondary processing, striking the surface of the intermediate workpiece or the intermediate blank so that the intermediate workpiece or the intermediate blank is completely fitted with the work surface.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The primary processing comprises: sequentially performing cutting and polishing on the intermediate workpiece; Preferably, the secondary processing comprises: polishing the intermediate blank; Preferably, the middle layer is circular or rectangular; Preferably, the thickness of the intermediate layer is 2.2 to 2.35 mm; Preferably, the roughness of the intermediate layer is ≤1.6 μm; Preferably, the flatness of the intermediate layer is ≤0.1 mm; Preferably, after the secondary processing is completed, the strong magnetic component is removed, and the first adhesive layer, the second adhesive layer and the third adhesive layer are scraped off.

10. The preparation method according to any one of claims 1 to 9, characterized in that: The intermediate workpiece is made of aluminum and / or titanium; Preferably, the purity of the intermediate workpiece is ≥ 99.6%.

Citation Information

Patent Citations

  • Method for welding brittle target material assembly

    CN113927117A

  • A CNC lathe fixing mechanism for machining titanium targets with good clamping effect

    CN215281014U