Preparation method of metal sulfide and application of metal sulfide in alkaline electrolyzed water
By forming iron and nickel bimetallic sulfides through interfacial reaction on the nickel mesh surface, the high efficiency, stability and preparation problems in the prior art are solved, and high-performance catalyst preparation under alkaline electrolytic water conditions is realized, and the simulation is shown Long-term stability and commercial application potential under industrial conditions.
Patent Information
- Application Number
- CN202411398872.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-29
AI Technical Summary
It is difficult to develop a simple, efficient and easy to amplify high-performance transition metal sulfide large-scale preparation method, and it is difficult to maintain long-term stability under alkaline electrolytic water conditions, which limits the efficiency and commercial application of electrolytic water hydrogen production technology.
Using KSCN as the sulfur source, by reacting trivalent iron ions and KSCN with elemental nickel in a weakly acidic aqueous solution, iron and nickel bimetallic sulfides are formed, and metal sulfides are formed in situ on the surface of the nickel mesh to avoid Complex preparation processes at high temperatures and high costs.
It achieves high activity and long-term stability under simulated industrial conditions (30% KOH, 80℃), and can operate stably for at least 160 hours at a current density of 1000 mA cm-2. The preparation method is simple and green, suitable for large Preparation of area catalyst.
Smart Images

Figure CN119040950A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-performance catalysts, and in particular to a method for preparing metal sulfide and application of the metal sulfide in alkaline electrolysis of water. Background Art
[0002] Hydrogen energy is a green and efficient energy carrier. Hydrogen production technology driven by electricity generated by renewable energy (such as solar and wind energy) has become a cutting-edge means for the efficient utilization and storage of intermittent renewable energy. The oxygen evolution reaction (OER) occurring at the anode is a bottleneck half-reaction that severely limits the overall efficiency of the electrolyzer due to its slow kinetics and thermodynamics. Therefore, the development of an electrocatalyst with both high activity and long-term stability is crucial to improve the reaction efficiency and reduce additional energy consumption. Transition metal-based compounds have been used as an efficient and economical alternative to precious metal-based catalysts. After several years of unremitting efforts, a large number of transition metal-based catalysts have been developed, such as transition metal oxides, (oxy)hydroxides, sulfides, selenides, phosphides and nitrides. Among them, transition metal sulfides have attracted widespread attention due to their low cost, abundant reserves, environmental friendliness and excellent electronic / chemical properties.
[0003] In order to prepare highly active metal sulfides, researchers have developed a variety of methods such as solvothermal and electrodeposition. However, these bottom-up preparation methods are relatively complex, time-consuming, and expensive, and are sometimes even accompanied by the production of toxic and harmful gases. In addition, it is difficult to achieve efficient preparation of large-area electrodes using these sophisticated preparation methods. The reported catalysts usually show good stability in a three-electrode system under laboratory conditions, and it is difficult to maintain long-term stability under harsh conditions of 30% KOH electrolyte solution, 80 °C high temperature, and thousands of milliamperes of current density, but this test environment is a prerequisite for commercial applications. Therefore, it is imperative to develop a simple, efficient, and easy-to-scale large-scale preparation method for high-performance transition metal sulfides, but it is also quite challenging. Summary of the invention
[0004] The purpose of the present invention is to provide a new method for preparing metal sulfide oxygen evolution quickly and greenly in view of the shortcomings of the prior art. The method can be used to prepare large-area catalysts at the square meter level. The metal sulfide exhibits excellent activity and stability (1000 mA cm -2 The current density should be stable for at least 160 h).
[0005] In the present invention, KSCN is used as a sulfur source, and trivalent iron ions and KSCN are first added to water and mixed evenly, wherein the molar ratio of the trivalent iron ions to KSCN is 2:3, and the concentration of the trivalent iron ions is 0.2-0.8 M; then elemental nickel is added, and after standing at room temperature, iron and nickel bimetallic sulfides can be obtained; the elemental nickel is excessive, and its molar amount is about 1:1 of Fe 3+ More than 4 times.
[0006] The trivalent iron ions of the present invention are derived from ferric nitrate and ferric chloride. The elemental nickel is added to the sulfur source in the form of nickel mesh, nickel sheet or nickel foam.
[0007] Specifically, the present invention adopts the following technical solution: the cleaned Ni mesh is immersed in Fe(NO 3 ) 3 6H 2 O and KSCN in a mixed solution at room temperature for 1 h, metal sulfides can be formed in situ on the Ni mesh surface through rapid interfacial reaction. 3 ) 3 6H 2 O in a weakly acidic aqueous solution, Fe 3+ Ions will react with NM to cause surface corrosion and cation dissolution; at the same time, SCN in aqueous solution - Hydrolysis to generate S 2- ions; finally, M δ+ With S 2- The ions react on the NM surface to form sulfide phases (M = Ni, Fe).
[0008] In some embodiments of the present invention, the following steps are included: (1) Nickel mesh (NM) was cut into strips of 2.0 cm × 2.0 cm and washed with acetone and 3 mol L -1 The samples were ultrasonically treated with hydrochloric acid for 10 min each, and then rinsed with deionized water (DI) and ethanol for 3 times, each time for 5 min. Then, the samples were taken out and dried naturally in the air overnight.
[0009] (2) Weigh 6 mmol Fe(NO 3 ) 3 6H 2 O and 9 mmol KSCN were added into 30 ml DI and stirred on a stirring table for 10 min until the solute was completely dissolved.
[0010] (3) Place a piece of NM in the above solution and let it stand for 1 hour. Then rinse the treated NM with DI and ethanol several times and dry it naturally in the air for 6 hours to obtain (Ni,Fe) loaded on the nickel mesh. x S y .
[0011] The invention also relates to the application of the metal sulfide in alkaline electrolyzed water.
[0012] The beneficial effects of the present invention are: 1. The preparation method of the present invention is simple, green and easy to scale up (500 × 500 mm); 2. The raw materials (Ni, Fe) used in the integrated electrode prepared by the present invention are naturally abundant and inexpensive; 3. Fe(NO 3 ) 3 6H 2 O aqueous solution is weakly acidic, oxygen corrosion can proceed spontaneously, no toxic or harmful gases are produced during the reaction, and the etching conditions are green and environmentally friendly.
[0013] 4. The integrated electrode prepared by the present invention can be directly used as a working electrode, effectively avoiding the agglomeration of active substances caused by the electrode preparation process; 5. The integrated electrode prepared by the present invention exhibits excellent stability under simulated industrial conditions (30% KOH, 80°C) and can -2 The device can operate stably for at least 160 h at a current density of 2.5 Å / s and has the potential for commercial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 (Ni,Fe) x S y Raman and XPS spectra of / NM. (a) Raman spectrum, (b) XPS spectrum.
[0015] Figure 2 (Ni,Fe) x S y SEM image of / NM and EDS element distribution map of the corresponding area.
[0016] Figure 3 (Ni,Fe) x S y Polarization curves of / NM. (a) Different Fe(NO 3 ) 3 6H 2 O molar concentration, (b) different KSCN molar concentrations, (c) different reaction times.
[0017] Figure 4 (Ni,Fe) x S y Stability curve of / NM / / NM in 30% KOH electrolyte, 80℃ and two-electrode system.
[0018] Figure 5 Optical images of NM before and after corrosion treatment. (a) Before treatment, (b) After treatment.
[0019] Figure 6 Scaled-up (Ni,Fe) x S y / NM SEM images and LSV curves of different regions. (ae) SEM images, (f) LSV curves of the corresponding regions. DETAILED DESCRIPTION
[0020] The following examples are used to further illustrate the present invention, and their purpose is to illustrate the present invention and should not be construed as limiting the scope of the present invention. Unless otherwise specified, all parts by weight and weight percentages are used below.
[0021] The raw materials used in the present invention, unless otherwise specified, are conventional commercially available products; the methods used in the present invention, unless otherwise specified, are conventional methods in the art.
[0022] Example 1 (1) Nickel mesh (NM) was cut into strips of 2.0 cm × 2.0 cm and washed with acetone and 3 mol L -1 The samples were ultrasonically treated with hydrochloric acid for 10 min each, and then rinsed with deionized water (DI) and ethanol for 3 times, each time for 5 min. Then, the samples were taken out and dried naturally in the air overnight.
[0023] (2) Weigh 6 mmol Fe(NO 3 ) 3 6H 2 O and 9 mmol KSCN were added into 30 ml DI and stirred on a stirring table for 10 min until the solute was completely dissolved.
[0024] (3) Place a piece of NM in the above solution and let it stand for 1 hour. Then rinse the treated NM with DI and ethanol several times and dry it naturally in the air for 6 hours to obtain (Ni,Fe) x S y / NM.
[0025] Figure 1 The (Ni,Fe) prepared in this example x S y Raman and XPS spectra of / NM. (Ni,Fe) x S y / NM at 230, 282, 377 and 455 cm -1The Raman characteristic peaks appeared at 162.2 eV and 163.6 eV in the high-resolution S 2p XPS spectrum, indicating the formation of a sulfide phase. In addition, the peaks at 168.7 eV were attributed to the sulfur oxide species produced by surface oxidation.
[0026] Figure 2 The (Ni,Fe) prepared in this example x S y / NM SEM image and EDS element distribution map of the corresponding area. It can be observed from the SEM image that after the rapid interface reaction, the originally smooth NM surface becomes rough and presents a cracked loose morphology, which is conducive to the penetration of the electrolyte and the exposure of the catalytic active sites, thereby greatly improving the catalytic performance. In addition, the EDS element distribution map shows that the Ni, Fe, S, and O elements in (Ni,Fe) x S y / NM is evenly distributed on the surface.
[0027] Figure 3 In this example, different Fe(NO 3 ) 3 6H 2 O and 9mmol KSCN concentration and reaction time to prepare (Ni,Fe) x S y In order to determine the feasible range of iron salts, the concentrations of iron salts and KSCN were increased simultaneously. First, under the conditions of constant molar concentration of KSCN and reaction time, the Fe(NO 3 ) 3 6H 2 The molar concentration of O was in the range of 0.2~0.8 M. The results showed that the concentration of iron salt had little effect on the performance of the catalyst. 3 ) 3 6H 2 Under the conditions of constant molar concentration of Fe(NO) and reaction time, the molar concentration of KSCN was adjusted in the range of 0.1~1.0 M. The results showed that with the increase of KSCN concentration, the catalytic performance first increased and then decreased, reaching the best under the condition of 0.3 M. Finally, under the condition of Fe(NO 3 ) 3 6H 2 Under the condition of constant molar concentration of O and KSCN, the reaction time was adjusted in the range of 10-180 min. The results showed that with the increase of reaction time, the catalytic performance first increased and then decreased, reaching the optimum under the condition of 60 min.
[0028] Figure 4The (Ni,Fe) prepared in this example x S y / NM stability test curve in 30% KOH electrolyte, 80℃, two-electrode system. Compared with NM / / NM, (Ni,Fe) prepared by this method x S y / NM assembled two-electrode system ((Ni,Fe) x S y / NM / / NM) exhibited excellent stability at 1000 mA cm -2 The device can stably operate at a current density of 1000 Å for at least 160 h, showing great potential for commercial applications.
[0029] Figure 5 This is the (Ni,Fe) prepared by enlarging the present embodiment. x S y Optical images of / NM, SEM images of different regions and LSV curves in 1M KOH electrolyte. It is particularly noted that this preparation method can be used for large-scale preparation. Due to the limitations of experimental conditions, we only carried out the scaled-up preparation with a size of 500×500 mm. After oxygen corrosion treatment, the NM, which originally had a silver-gray metallic luster on the surface, turned into a uniform black appearance.
[0030] Figure 6 It is a scaled-up preparation (Ni,Fe) x S y / NM SEM images and LSV curves of different regions. SEM images of randomly selected regions 1#-5# show similar morphology ( Figure 6 ae), indicating that the microstructure of the large-area electrode is the same. Meanwhile, regions 1#-5# exhibit similar OER activities in the three-electrode system ( Figure 6 f), further supports this claim.
[0031] Example 2 (1) A 2.0 cm × 2.0 cm nickel foam was prepared by acetone and 3 mol L -1 The samples were ultrasonically treated with hydrochloric acid for 10 min each, and then rinsed with deionized water (DI) and ethanol for 3 times, each time for 5 min. Then, the samples were taken out and dried naturally in the air overnight.
[0032] (2) Weigh 6 mmol Fe(NO 3 ) 3 6H 2 O and 9 mmol KSCN were added into 30 ml DI and stirred on a stirring table for 10 min until the solute was completely dissolved.
[0033] (3) Place the nickel foam in the above solution and let it stand for 1 hour. Then rinse the treated nickel foam with DI and ethanol several times and dry it naturally in the air for 6 hours to obtain (Ni,Fe) loaded on the nickel foam. x S y .
[0034] Characterization was performed according to the characterization methods of the embodiment. Raman and XPS results showed that a sulfide phase was also formed in the product of this embodiment. At the same time, the SEM image also showed the same crack morphology, and the corresponding EDS element distribution diagram revealed that the elements Ni, Fe, S, and O were evenly distributed. In addition, the catalyst prepared by this method also showed excellent catalytic performance under the conditions of 30% KOH electrolyte, 80°C, and a two-electrode system.
[0035] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.
Claims
1. A method for preparing metal sulfide, characterized in that: Taking KSCN as a sulfur source, first add trivalent iron ions and KSCN into water and mix them evenly, wherein the molar ratio of the trivalent iron ions to KSCN is 2:3, and the concentration of the trivalent iron ions is 0.2-0.8 M; then add elemental nickel, and after standing at room temperature, iron and nickel bimetallic sulfides can be obtained; the elemental nickel is excessive, and its molar amount is about 1.5-2.0 moles per 100 t of Fe 3+ More than 4 times.
2. The preparation method according to claim 1, characterized in that: The trivalent iron ions are derived from ferric nitrate and ferric chloride.
3. The preparation method according to claim 1, characterized in that: The elemental nickel is added to the sulfur source in the form of a nickel mesh, a nickel sheet or a nickel foam.
4. Use of the metal sulfide prepared by the method according to any one of claims 1 to 3 in alkaline electrolyzed water.