Carbon fiber material, preparation method and application thereof

By preparing Ni(SeMo)OX active components on carbon fiber materials, combined with vibration control technology, a catalyst with a triangular sheet-like structure is formed, which solves the problem of slow kinetics and high overpotentiality of the water cracking electrocatalyst, and achieves low cost and high efficiency The electrolytic aquatic hydrogen reaction demonstrates the great potential of carbon fiber materials in the field of electrocatalysis.

CN119040984APending Publication Date: 2024-11-29郭洪菲
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411230369.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the slow kinetics and high overpotential of water cracking electrocatalysts limit the practical application of water splitting. Traditional hydrogen preparation methods rely on non-renewable fossil fuels, and the development of carbon-based materials in the field of electrocatalytics has not yet fully utilized. potential.

Method used

Using carbon fiber material as the substrate, Ni(SeMo)OX active components are prepared by multiphase pulse electrodeposition technology, combined with the vibration control of flexible carbon fiber film and rigid polyurethane resin rods, forming a catalyst with a triangular sheet-like structure to achieve low overpotential and High catalytic activity.

Benefits of technology

The electrolytic aquatic hydrogen reaction with low overpotential (only 80mV) and high current density (10mA/cm2) is achieved, which improves the efficiency of converting electrical energy into chemical energy, has industrial application potential, and shows excellent electrochemical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides a carbon fiber material and a preparation method and application thereof.A flexible carbon fiber film is fixed to the surface of a hard polyurethane resin rod in a wrapping mode, the carbon fiber film serves as a cathode, vibration control of the cathode is assisted, Ni (SeMo) OX active components are effectively and electrically deposited on the surface of carbon fiber, the active components are of a triangular sheet structure, and therefore the carbon fiber material has a good anti-corrosion effect on the surface of the carbon fiber; the carbon fiber material with the Ni (SeMo) OX active component loaded on the surface has excellent hydrogen evolution activity and low hydrogen evolution overpotential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical industry, and specifically relates to a carbon fiber material, a preparation method and application thereof. Background Art

[0002] As people realize the seriousness of environmental pollution and the reduction of fossil energy that cannot be regenerated in a short period of time, as well as the energy crisis and more serious environmental pollution caused by the continuous depletion of limited fossil fuels, many scientists are currently developing clean, effective and low-cost renewable energy, which is an important step to achieve green and sustainable development. This has also aroused great attention from researchers and researchers to clean and renewable energy alternatives. These green renewable energy sources include hydrogen energy, nuclear energy, wind power, hydropower, thermal power and bioenergy. Hydrogen energy is a resource with rich thermal energy and clean and pollution-free. At the same time, the source of hydrogen production is very simple and easy to obtain. Since there are abundant water resources in the world, water is an important source of hydrogen, which makes hydrogen have great development potential to become an important resource in the future. Hydrogen can be regarded as an environmentally friendly and safe renewable energy source because of its large thermal energy volume and convenient transportation, and water is its main product. Hydrogen is considered one of the most promising new energy sources in the 21st century, and electrochemical hydrogen production is considered an ideal candidate for further energy supply. Through the research of scientists, it is found that the cracking of water is mainly composed of two chemical reactions, and the reaction requires a theoretical potential of 1.23V. However, the slow kinetics and high overpotential of HER and OER still limit the practical application of overall water splitting to date. Scientists have verified that platinum alloys and ruthenium iridium oxides exhibit ideal HER and OER activities, respectively. However, due to the scarcity and high cost of alloys, platinum alloys and ruthenium iridium oxides are basically not used. Therefore, finding the required water splitting electrocatalyst is an urgent task. The traditional way to prepare hydrogen is to obtain hydrogen by consuming non-renewable fossil fuels, but the hydrogen prepared by this method has low utilization rate and low purity, which greatly reduces the efficiency of industrial production. In contrast, the preparation of hydrogen by electrochemical splitting of water can fully meet industrial needs and has certain application value among the many methods of preparing hydrogen.

[0003] Carbon-based materials are common electrocatalyst substrates, and the method of loading transition metal atoms is usually used to improve the HER electrocatalytic activity. Compared with common metal-based catalysts, carbon-based materials have the following advantages: (1) Low cost. Carbon-based materials are abundant and cheap, and can be easily synthesized from various sources such as coal and petroleum. (2) High specific surface area. Carbon-based electrocatalysts have a high specific surface area, which is attributed to their porous structure. The pore size can be controlled by the synthesis conditions, providing more active sites and possibilities for electrochemical reactions. (3) Adjustable electronic properties. Carbon-based materials can exhibit different electronic properties through functionalization of functional groups or incorporation of heteroatoms, making their electrocatalytic activity highly adjustable. (4) High chemical stability. Carbon-based materials are inert in acidic and alkaline environments, can react under harsh conditions, and maintain electrochemical activity for a long time. Carbon-based materials have many advantages in the field of electrocatalysis and are considered to be one of the most promising electrocatalyst carriers.

[0004] For example, CN112708904A discloses a preparation method and application of a carbon fiber-supported nano-cobalt-molybdenum alloy catalyst. The present invention uses carbon fiber paper as a base material, sodium hydroxide, sodium citrate, a cobalt source and a molybdenum source as raw materials, and adopts a multiphase pulse electrodeposition technology to obtain the target material. The preparation method of the present invention is simple and controllable, with a short preparation cycle, low production cost, good repeatability, and is very likely to achieve large-scale production. Benefiting from its own advantages such as large specific surface area, good electrical conductivity, and strong adhesion between the cobalt-molybdenum alloy and the substrate, the obtained cobalt-molybdenum nano-alloy material can be used in an alkaline electrolytic cell to electrolyze water to produce hydrogen. The optimal overpotential of only 80mV is required to achieve a current density of 10mAcm 2 The ability to efficiently catalyze the electrolysis of water to produce hydrogen over an extremely long period of time can greatly improve the energy conversion efficiency of converting electrical energy into chemical energy and has potential industrial applications.

[0005] For example, CN118127554A discloses a carbon fiber cloth-supported transition metal catalyst and its preparation method and application, including: first, growing a NiFeCe-LDH nanosheet precursor on a carbon fiber cloth substrate using a hydrothermal method; and secondly, preparing a Fe-Ni2P / CeO2 product using a low-temperature phosphating reaction. The present invention utilizes the synergy and uniform nanosheet structure between Fe-Ni2P and CeO2 to regulate the electronic structure of the catalyst and expose abundant active sites, thereby achieving the goal of reducing the reaction energy barrier. When the present invention is applied to the process of preparing hydrogen by electrolysis of water, it exhibits high catalytic activity and cyclic stability, and only a relatively low voltage of 1.554V needs to be applied to achieve 10mA / cm 2 The synthesis process of the present invention is simple to operate and has low cost, and can be used as an efficient catalyst for hydrogen production by electrolysis of water.

[0006] For example, CN104674297A discloses a method for preparing a transition metal sulfide compound hydrogen evolution electrode, comprising the following preparation steps: dispersing two-dimensional transition metal sulfide compound nanosheets into a mixture of water and anhydrous ethanol to prepare a transition metal sulfide compound nanosheet suspension having a mass concentration of 0.01 to 5 g / L; depositing the nanosheet suspension onto a carbon cloth by electrophoresis; during the electrophoresis process, a stainless steel plate is connected to the negative electrode of a DC power supply, and the carbon cloth is connected to the positive electrode of the DC power supply, with a voltage of 50 to 200 V and a spacing of 0.3 to 2 cm between the two electrodes; drying the carbon cloth treated by electrophoresis in step (2) at 55 to 70° C. for 12 to 24 hours, and then calcining at 140 to 160° C. for 0.5 to 5 hours to prepare a hydrogen evolution electrode material. The method of the present invention is simple and easy to implement, has low production cost, and can be used not only in industrial electrocatalytic hydrogen production, but also in various catalytic hydrogen evolution fields, such as solar water electrolysis for hydrogen production. Summary of the invention

[0007] The present invention provides a carbon fiber material, a preparation method and an application thereof, wherein a flexible carbon fiber film is coated and fixed on the surface of a hard polyurethane resin rod, and the carbon fiber film is used as a cathode to assist in the vibration control of the cathode itself, thereby effectively electrodepositing Ni(SeMo)O on the surface of the carbon fiber. X The active component presents a triangular sheet structure, and the surface is loaded with Ni(SeMo)O X The carbon fiber material of the active component has excellent hydrogen evolution activity and low hydrogen evolution overpotential, which is mainly attributed to the catalytic activity of the active component, the high specific surface area of ​​the carrier, the morphology and structure of the active component, and the excellent conductivity. In addition, the carbon fiber material of the present invention has excellent electrochemical hydrogen evolution stability.

[0008] A method for preparing a carbon fiber material comprises the following steps: (1) Cut the carbon fiber film into sheets and place them in a mixture of acetone and ethanol organic solvents for ultrasonic cleaning; transfer the cleaned carbon fiber cloth into a potassium permanganate solution for soaking; then soak and clean it with ethanol and blow dry with cold air; (2) cleaning the surface of the hard polyurethane resin rod, and wrapping the flexible carbon fiber membrane obtained by the pretreatment in step (1) on the surface of the hard polyurethane resin rod by multiple layers, and fixing it up and down with stainless steel wire; (3) Combine SeO2, Ni(NO3)2 . 6H2O、(NH4)6Mo7O 24 . 4H2O, H3BO4, Na2SO4, C 12 H 25 SO4Na and EDTA-Na were dissolved in deionized water, stirred evenly, and the pH value was adjusted to prepare an electrolyte. (4) The end of the rigid polyurethane resin rod coated with the flexible carbon fiber membrane is immersed in the electrolyte, and the other end is connected to the vibration controller; one end of the stainless steel wire extends out of the electrolyte and is connected to the power supply as the cathode; (5) Control the frequency and amplitude of the vibration controller; control the power supply to implement electrodeposition; (6) Disconnect the power supply and the vibration controller, disassemble the stainless steel wire, remove the flexible carbon fiber membrane, perform heat treatment, and cool naturally to obtain the carbon fiber material.

[0009] Step (1) cutting the carbon fiber film into 4-5*6-10 cm sheets, placing it in a mixed solution of acetone and ethanol organic solvent with a volume ratio of 1:1-2 and ultrasonically cleaning it for 0.5-3 hours; transferring the cleaned carbon fiber cloth into a 5-7wt.% potassium permanganate solution and soaking it for 1-1.5 hours at a reaction temperature of 70-80°C; then soaking and cleaning it in ethanol for 10-20 minutes, and blowing it dry with cold air.

[0010] The radius of the hard polyurethane resin rod is 0.25-0.5 cm, and a fixing groove for the stainless steel wire is arranged on the surface of the hard polyurethane resin rod.

[0011] Electrolyte preparation: 2-3g SeO2, 10-12g Ni(NO3)2 . 6H2O, 8-10g (NH4)6Mo7O 24 . 4H2O, 4-5gH3BO4, 2-3g Na2SO4, 0.05-0.1g C 12 H 25 SO4Na and 1-2g EDTA-Na were dissolved in deionized water.

[0012] pH=5.5-6.5.

[0013] Control the frequency of the vibration controller to 40-60KHz.

[0014] Control the power supply voltage to 8-10V, the time to 10-20min, and the temperature to 3-7℃.

[0015] Heat treatment: Place in air atmosphere, heat treatment at 200-300℃ for 10-15min, switch gas path, heat treatment at 400-450℃ for 20-30min in 3-5vol.%H2 / Ar atmosphere.

[0016] The carbon fiber has a size of 200-400 nm and has triangular flake-like Ni(SeMo)O X , for hydrogen evolution cathode applications.

[0017] Technical effects: (1) The carrier substrate used in the present invention is a carbon fiber membrane, which has good flexibility and electrical conductivity and is suitable for electrode materials with high catalytic hydrogen evolution; (2) By controlling the vibration frequency of the carbon fiber, a catalytic material with a high specific surface area is prepared. The carbon fiber catalytic material has a high charge transfer rate and a low hydrogen evolution overpotential. The active area is efficiently exposed by adjusting the vibration frequency, showing excellent catalytic hydrogen evolution performance by electrolysis of water; (3) Ni(SeMo)O with a triangular sheet structure is electrochemically deposited. X Easy for gas diffusion and precipitation; (4) Cathode vibration is beneficial to the catalytic stability of carbon fiber membrane catalytic materials when used in the field of water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Attached Figure 1 LSV polarization curves of different embodiments and comparative example 1.

[0019] Attached Figure 2 Tafel slopes of different embodiments and Comparative Example 1.

[0020] Attached Figure 3 Impedance curves of different embodiments and comparative example 1.

[0021] Attached Figure 4 Cyclic voltammetry curve of Comparative Example 1.

[0022] Attached Figure 5 Cyclic voltammetry curve of Example 3.

[0023] Attached Figure 6 Stability testing. DETAILED DESCRIPTION Example 1

[0024] A method for preparing a carbon fiber material comprises the following steps: (1) Cut the carbon fiber membrane into sheets and place them in a mixture of acetone and ethanol organic solvents with a volume ratio of 1:1 for ultrasonic cleaning for 0.5 h; transfer the cleaned carbon fiber cloth to a 5wt.% potassium permanganate solution for oxidation treatment and soak it for 1 h at a reaction temperature of 70°C; then soak it in ethanol for 10 min and blow dry it with cold air.

[0025] (2) The hard polyurethane resin rod is surface cleaned, and the flexible carbon fiber membrane obtained by the pretreatment in step (1) is wrapped around the surface of the titanium alloy metal rod in multiple layers, and fixed up and down with stainless steel wire.

[0026] (3) 2g SeO2, 10g Ni(NO3)2 . 6H2O, 8g(NH4)6Mo7O 24 . 4H2O, 4gH3BO4, 2gNa2SO4, 0.05gC12 H 25 SO4Na and 1g EDTA-Na were dissolved in deionized water, stirred evenly, and the pH was adjusted to 5.5 to prepare an electrolyte.

[0027] (4) The rigid polyurethane resin rod coated with the flexible carbon fiber membrane is immersed in the electrolyte, and the other end is connected to the vibration controller; one end of the stainless steel wire extends out of the electrolyte and is connected to the power supply as the cathode.

[0028] (5) Control the frequency of the vibration controller to 40KHz; control the power supply voltage to 8V, the time to 10min, and the temperature to 3℃.

[0029] (6) Disconnect the power supply and vibration controller, disassemble the stainless steel wire, remove the flexible carbon fiber membrane, place it in an air atmosphere, heat treat it at 200°C for 10 min, switch the gas path, heat treat it at 400°C for 20 min in a 3 vol.% H2 / Ar atmosphere, and cool it naturally to obtain the carbon fiber material. Example 2

[0030] A method for preparing a carbon fiber material comprises the following steps: (1) Cut the carbon fiber membrane into sheets and place them in a mixture of acetone and ethanol organic solvents with a volume ratio of 1:1.5 for ultrasonic cleaning for 2.5 hours; transfer the cleaned carbon fiber cloth to a 7wt.% potassium permanganate solution for oxidation treatment and soak it for 1.25 hours at a reaction temperature of 75°C; then soak it in ethanol for 15 minutes and blow dry it with cold air.

[0031] (2) The hard polyurethane resin rod is surface cleaned, and the flexible carbon fiber membrane obtained by the pretreatment in step (1) is wrapped around the surface of the titanium alloy metal rod in multiple layers, and fixed up and down with stainless steel wire.

[0032] (3) 2.5g SeO2, 11g Ni(NO3)2 . 6H2O, 9g(NH4)6Mo7O 24 . 4H2O, 4.5gH3BO4, 2.5gNa2SO4, 0.075g C 12 H 25 SO4Na and 1.5g EDTA-Na were dissolved in deionized water, stirred evenly, and the pH was adjusted to 6 to prepare an electrolyte.

[0033] (4) The rigid polyurethane resin rod coated with the flexible carbon fiber membrane is immersed in the electrolyte, and the other end is connected to the vibration controller; one end of the stainless steel wire extends out of the electrolyte and is connected to the power supply as the cathode.

[0034] (5) Control the frequency of the vibration controller to 45KHz; control the power supply voltage to 9V, the time to 15min, and the temperature to 5℃.

[0035] (6) Disconnect the power supply and vibration controller, disassemble the stainless steel wire, remove the flexible carbon fiber membrane, place it in an air atmosphere, heat treat it at 250°C for 12.5 min, switch the gas path, heat treat it at 425°C for 25 min in a 4 vol.% H2 / Ar atmosphere, and cool it naturally to obtain the carbon fiber material. Example 3

[0036] A method for preparing a carbon fiber material comprises the following steps: (1) Cut the carbon fiber membrane into sheets and place them in a mixture of acetone and ethanol organic solvents with a volume ratio of 1:1.5 for ultrasonic cleaning for 2.5 hours; transfer the cleaned carbon fiber cloth to a 7wt.% potassium permanganate solution for oxidation treatment and soak it for 1.25 hours at a reaction temperature of 75°C; then soak it in ethanol for 15 minutes and blow dry it with cold air.

[0037] (2) The hard polyurethane resin rod is surface cleaned, and the flexible carbon fiber membrane obtained by the pretreatment in step (1) is wrapped around the surface of the titanium alloy metal rod in multiple layers, and fixed up and down with stainless steel wire.

[0038] (3) 2.5g SeO2, 11g Ni(NO3)2 . 6H2O, 9g(NH4)6Mo7O 24 . 4H2O, 4.5gH3BO4, 2.5gNa2SO4, 0.075g C 12 H 25 SO4Na and 1.5g EDTA-Na were dissolved in deionized water, stirred evenly, and the pH was adjusted to 6 to prepare an electrolyte.

[0039] (4) The rigid polyurethane resin rod coated with the flexible carbon fiber membrane is immersed in the electrolyte, and the other end is connected to the vibration controller; one end of the stainless steel wire extends out of the electrolyte and is connected to the power supply as the cathode.

[0040] (5) Control the frequency of the vibration controller to 50KHz; control the power supply voltage to 9V, the time to 15min, and the temperature to 5℃.

[0041] (6) Disconnect the power supply and vibration controller, disassemble the stainless steel wire, remove the flexible carbon fiber membrane, place it in an air atmosphere, heat treat it at 250°C for 12.5 min, switch the gas path, heat treat it at 425°C for 25 min in a 4 vol.% H2 / Ar atmosphere, and cool it naturally to obtain the carbon fiber material. Example 4

[0042] A method for preparing a carbon fiber material comprises the following steps: (1) The carbon fiber membrane was cut into sheets and ultrasonically cleaned in a mixture of acetone and ethanol in a volume ratio of 1:2 for 3 h; the cleaned carbon fiber cloth was transferred to a 7 wt.% potassium permanganate solution for oxidation treatment and soaked for 1.5 h at a reaction temperature of 80 °C; then, it was soaked and cleaned in ethanol for 20 min and dried with cold air.

[0043] (2) The hard polyurethane resin rod is surface cleaned, and the flexible carbon fiber membrane obtained by the pretreatment in step (1) is wrapped around the surface of the titanium alloy metal rod in multiple layers, and fixed up and down with stainless steel wire.

[0044] (3) 3g SeO2, 12g Ni(NO3)2 . 6H2O, 10g(NH4)6Mo7O 24 . 4H2O, 5gH3BO4, 3gNa2SO4, 0.1gC 12 H 25 SO4Na and 2g EDTA-Na were dissolved in deionized water, stirred evenly, and the pH was adjusted to 6.5 to prepare an electrolyte.

[0045] (4) The rigid polyurethane resin rod coated with the flexible carbon fiber membrane is immersed in the electrolyte, and the other end is connected to the vibration controller; one end of the stainless steel wire extends out of the electrolyte and is connected to the power supply as the cathode.

[0046] (5) Control the frequency of the vibration controller to 60KHz; control the power supply voltage to 10V, the time to 20min, and the temperature to 7℃.

[0047] (6) Disconnect the power supply and vibration controller, disassemble the stainless steel wire, remove the flexible carbon fiber membrane, place it in an air atmosphere, heat treat it at 300°C for 15 min, switch the gas path, heat treat it at 450°C for 30 min in a 5 vol.% H2 / Ar atmosphere, and cool it naturally to obtain the carbon fiber material.

[0048] Comparative Example 1: A method for preparing a carbon fiber material, comprising the following steps: (1) Cut the carbon fiber membrane into sheets and place them in a mixture of acetone and ethanol organic solvents with a volume ratio of 1:1.5 for ultrasonic cleaning for 2.5 hours; transfer the cleaned carbon fiber cloth to a 7wt.% potassium permanganate solution for oxidation treatment and soak it for 1.25 hours at a reaction temperature of 75°C; then soak it in ethanol for 15 minutes and blow dry it with cold air.

[0049] (2) The hard polyurethane resin rod is surface cleaned, and the flexible carbon fiber membrane obtained by the pretreatment in step (1) is wrapped around the surface of the titanium alloy metal rod in multiple layers, and fixed up and down with stainless steel wire.

[0050] (3) 2.5g SeO2, 11g Ni(NO3)2 . 6H2O, 9g(NH4)6Mo7O 24 . 4H2O, 4.5gH3BO4, 2.5gNa2SO4, 0.075g C 12 H 25 SO4Na and 1.5g EDTA-Na were dissolved in deionized water, stirred evenly, and the pH was adjusted to 6 to prepare an electrolyte.

[0051] (4) The rigid polyurethane resin rod coated with the flexible carbon fiber membrane is immersed in the electrolyte, and the other end is connected to the vibration controller; one end of the stainless steel wire extends out of the electrolyte and is connected to the power supply as the cathode.

[0052] (5) The vibration controller is controlled not to work. Instead, an electrolytic cell with ultrasonic function is used to apply a vibration frequency of 50 kHz to the bottom of the electrolytic cell, similar to ultrasonic stirring; the control power supply voltage is 9 V, the time is 15 min, and the temperature is 5 °C.

[0053] (6) Disconnect the power supply and vibration controller, disassemble the stainless steel wire, remove the flexible carbon fiber membrane, place it in an air atmosphere, heat treat it at 250°C for 12.5 min, switch the gas path, heat treat it at 425°C for 25 min in a 4 vol.% H2 / Ar atmosphere, and cool it naturally to obtain the carbon fiber material.

[0054] The electrochemical performance tests were performed on the embodiments of the present invention and the comparative examples.

[0055] Electrochemical tests were performed on a CHI 660E workstation using a three-electrode system, with the prepared catalyst as the working electrode, calomel electrode (SCE) as the reference electrode, and Pt as the counter electrode. The electrolytic cell for the hydrogen evolution reaction was made of glass material and the electrolyte was 1.0 M KOH. All potentials were converted to reversible hydrogen electrode potentials according to the Nernst equation.

[0056] The principle of Linear Sweep Voltammetry (LSV) is to apply a certain voltage to the working electrode and detect the change of potential and time. It is a technique for recording the change of current as the electrode potential changes, and the resulting curve is the linear sweep voltammogram. The carbon fiber materials prepared in the embodiments and comparative examples were used to electrolyze water to produce hydrogen, and the electrochemical properties of the carbon fiber electrodes were tested using a three-electrode system, and the voltage drop (IR) automatic compensation was selected in the electrochemical workstation. The carbon fibers prepared in the embodiments and comparative examples were used as working electrodes, platinum wire as the counter electrode, and saturated calomel electrode as the reference electrode for testing in KOH solutions of the same concentration.

[0057] Stability test: The carbon fiber material was placed in 1.0 M KOH for a certain period of cyclic voltammetry scanning, and the number of cycles was set to 6000. The hydrogen evolution polarization curve was tested, and the hydrogen evolution polarization curves before and after the cycle were compared to compare the hydrogen evolution overpotential before and after the cycle.

[0058] Electrochemical AC impedance: After applying a disturbance signal of a certain magnitude to the electrode system, an AC impedance spectrum is obtained that can represent the relationship between the response and the disturbance signal. The equivalent circuit is inferred from the AC impedance diagram. The resistance generated by the charge transfer process is inferred from the equivalent circuit, and the catalytic effect of the carbon fiber material is verified based on the size of the resistance.

[0059] The polarization of the electrode reflects the obstruction of the electrode process. The relationship between the current density and the overpotential under the electrode working conditions is plotted in a semi-logarithmic manner. After selective fitting of the graph, the slope of a straight line can be obtained. This is the Tafel slope graph, which reflects the degree to which the potential of the carbon fiber needs to change in order to achieve a specific current density.

[0060] See attached Figure 1 The LSV polarization curves of Examples 1-4 and Comparative Example 1 in 1 MKOH are shown. It can be seen that D-1, S-1, S-4, S-3, and S-2 have a high conductivity at 10 mA / cm 2 The overpotentials of hydrogen evolution are 241 mV, 162 mV, 139 mV, 121 and 181 mV respectively, among which Example 3 shows the best HER activity. In order to better determine the kinetic rate-controlling step of the composite material in the electrocatalytic water decomposition hydrogen process, the LSV polarization curve obtained in this experiment was subjected to Tafel slope fitting processing, see Appendix Figure 2 The Tafel slope values ​​of D-1, S-1, S-4, S-3, and S-2 are 149 mV / dec, 158 mV / dec, 139 mV / dec, 119 mV / dec, and 113 mV / dec, respectively. Figure 3Example 3 has a relatively smaller charge transfer resistance. The carbon fiber membrane catalytic material prepared in Example 3 has a faster charge transfer rate in the electrocatalytic water decomposition hydrogen process. Figure 4 and attached Figure 5 The double-layer capacitance of the carbon fiber membrane can be obtained from the cyclic voltammetry test results at different scan rates. The double-layer capacitance of Example 3 is 4.55 mF / cm 2 In comparison, the double layer capacitance of Comparative Example 1 is 1.05 mF / cm 2 The electrochemical active area of ​​a material known to those skilled in the art is proportional to the double-layer capacitance of the material. The only difference between Example 3 and Comparative Example 1 is that, under the premise of cathode vibration or electrolyte vibration, Example 3 has the largest electrochemical active area. Figure 6 After 6000 cycles of cyclic voltammetry test, the LSV polarization curve comparison before and after the test shows that the carbon fiber membrane of Example 3 did not show a significant decrease after 6000 cycles of CV cycle test. 2 The hydrogen evolution overpotential at the current density was only increased by 28 mV, that is, Example 3 has better electrocatalytic water decomposition hydrogen stability performance. In comparison, the comparative example 1 has a lower current density at 10 mA / cm 2 The hydrogen evolution overpotential under current density increased by 94 mV, and the stability was poor. The surface of the cleaned and oxidized carbon fiber was smooth and the size of the carbon fiber was 200-400nm; after electrochemical deposition treatment, the active components on the surface of the carbon fiber were similar to triangular flakes, and the structure was conducive to hydrogen evolution. In comparison, the material obtained in Comparative Example 1 had no triangular flake structure on the surface, but a disorderly stacked particle morphology.

[0061] The above embodiments are descriptions of specific implementation methods of the present invention rather than limitations of the present invention. Technical personnel in the relevant technical field can make various changes and modifications to obtain corresponding equivalent technical solutions without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions should be included in the patent protection scope of the present invention.

Claims

1. A method for preparing a carbon fiber material, characterized in that The steps include: (1) Cut the carbon fiber membrane into sheets and place them in a mixture of acetone and ethanol organic solvents for ultrasonic cleaning; transfer the cleaned carbon fiber cloth to a potassium permanganate solution for soaking; then soak and clean it with ethanol and blow dry with cold air; (2) Cleaning the surface of the rigid polyurethane resin rod, and wrapping the flexible carbon fiber membrane obtained in the pretreatment of step (1) on the surface of the rigid polyurethane resin rod by multiple layers, and fixing it up and down with stainless steel wire; (3) Combine SeO2, Ni(NO3)2 . 6H2O, (NH4)6Mo7O 24 . 4H2O, H3BO4, Na2SO4, C 12 H 25 SO4Na and EDTA-Na were dissolved in deionized water, stirred evenly, and the pH value was adjusted to prepare the electrolyte. (4) The rigid polyurethane resin rod coated with a flexible carbon fiber membrane is immersed in the electrolyte, and the other end is connected to the vibration controller; one end of the stainless steel wire extends out of the electrolyte and is connected to the power supply as the cathode; (5) Control the frequency and amplitude of the vibration controller; Controlling power supply to implement electrodeposition; (6) Disconnect the power supply and vibration controller, disassemble the stainless steel wire, remove the flexible carbon fiber membrane, perform heat treatment, and cool naturally to obtain the carbon fiber material.

2. The method for preparing a carbon fiber material according to claim 1, wherein Step (1) cutting the carbon fiber membrane into 4-5*6-10 cm sheets, placing it in a mixture of acetone and ethanol organic solvents with a volume ratio of 1:1-2 and ultrasonically cleaning it for 0.5-3 hours; transferring the cleaned carbon fiber cloth into a 5-7wt.% potassium permanganate solution and soaking it for 1-1.5 hours at a reaction temperature of 70-80°C; then soaking and cleaning it in ethanol for 10-20 minutes and blowing it dry with cold air.

3. The method for preparing a carbon fiber material according to claim 1, wherein The radius of the hard polyurethane resin rod is 0.25-0.5 cm, and a fixing groove for the stainless steel wire is provided on the surface of the hard polyurethane resin rod.

4. The method for preparing a carbon fiber material according to claim 1, wherein 2-3g SeO2, 10-12g Ni(NO3)2 . 6H2O, 8-10g (NH4)6Mo7O 24 . 4H2O, 4-5g H3BO4, 2-3g Na2SO4, 0.05-0.1g C 12 H 25 SO4Na and 1-2g EDTA-Na were dissolved in deionized water.

5. The method for preparing a carbon fiber material according to claim 1, wherein pH=5.5-6.

5.

6. The method for preparing a carbon fiber material according to claim 1, wherein Control the frequency of the vibration controller to 40-60KHz.

7. The method for preparing a carbon fiber material according to claim 1, wherein Control the power supply voltage to 8-10V, the time to 10-20min, and the temperature to 3-7℃.

8. The method for preparing a carbon fiber material according to claim 1, wherein Place in air atmosphere, heat treatment at 200-300℃ for 10-15min, switch gas path, heat treatment at 400-450℃ for 20-30min in 3-5vol.% H2 / Ar atmosphere.

9. A carbon fiber material, characterized in that The carbon fiber is obtained by the preparation method according to any one of claims 1 to 8, and the size of the carbon fiber is 200-400 nm, and a triangular sheet of Ni(SeMo)O is attached to the surface. X .

10. An application of carbon fiber material, characterized in that Application of the carbon fiber material according to claim 9 or the carbon fiber material obtained by the preparation method according to any one of claims 1 to 8 as a hydrogen evolution cathode.

Citation Information

Cited By

  • Preparation method and application of industrial-oriented alkaline hydrogen production difunctional electrode

    CN121228313A

  • Preparation method of alkaline hydrogen production bifunctional electrode for industrialization and application thereof

    CN121228313B