Electrophoresis process for producing and processing new energy automobile parts
The electrophoresis process used in the production and processing of new energy vehicle parts has solved the problems of poor coating quality and efficiency, achieved uniformity and corrosion resistance of the electrophoretic layer, adapted to automated production line operations, reduced production costs, and met environmental protection requirements.
Patent Information
- Application Number
- CN202411143291.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
AI Technical Summary
The coating quality and efficiency of existing new energy vehicle parts are not good. Cathodic electrophoretic coating has problems such as complex process, high cost and environmental non-environmental protection.
An electrophoresis process for the production and processing of new energy vehicle parts is adopted, which includes steps such as placement, degreasing, first water washing, phosphating treatment, second water washing, electrophoresis and baking. The electrophoresis temperature and bath parameters are strictly controlled to ensure that the electrophoretic layer is uniform in thickness and highly stable, reduce the evaporation of the bath solvent, and improve the electrophoresis quality.
It improves coating quality and efficiency, has strong adhesion and good corrosion resistance of the electrophoretic layer, meets environmental protection requirements, reduces production costs, and is suitable for automated production line operations.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of automobile parts processing, in particular to an electrophoresis process for producing and processing new energy automobile parts. Background Art
[0002] In recent years, the automobile manufacturing industry has developed rapidly. While production and sales continue to rise, auto parts are affected by the working environment and are subject to impact from sand and gravel and erosion from dirt such as mud and water on the ground. Therefore, high requirements are placed on the surface coating. After phosphating and then dip-coating with water-based epoxy primer, different degrees of rust and blistering were found in the car after one year of use. People have put forward higher quality requirements on the coating performance and corrosion resistance of automobile-related parts.
[0003] After using cathodic electrophoretic coating, the corrosion resistance of the workpiece is greatly improved, and the coating can withstand salt spray for up to 500 hours, which greatly extends the service life of the workpiece. Compared with previous dipping and spraying, electrophoretic coating is much more complicated.
[0004] At present, there are many automobile parts manufacturers, and the coating technology varies greatly. In addition, the main problems of the zinc-nickel-manganese ternary phosphating solution used in cathodic electrophoretic coating are: high working temperature and much phosphating sludge; complex component ratio, narrow process parameter range, and difficulty in control; high nickel and manganese content in the phosphating solution, high cost, poor market competitiveness, and both nickel and manganese are toxic heavy metals, which are not conducive to environmental protection; slow phosphating speed, not suitable for automatic coating line operation, affecting the coating quality and efficiency in automobile parts production, so an electrophoretic process for the production and processing of new energy automobile parts is proposed to solve the above problems. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the shortcomings of the prior art, the present invention provides an electrophoretic process for the production and processing of new energy vehicle parts, which has the advantages of improving coating quality and efficiency, and solves the problems of poor coating quality and efficiency.
[0007] (II) Technical solution
[0008] In order to achieve the above-mentioned purpose of improving the coating quality, the present invention provides the following technical solution: an electrophoresis process for the production and processing of new energy vehicle parts, comprising the following steps:
[0009] S1. Placement: Hang the parts on a special rack, hang them firmly and securely, and polish the contact points between the rack and the parts until the metallic luster is exposed to ensure good conductivity;
[0010] S2. Degreasing: As parts are usually protected with anti-rust grease during storage and transportation, there are often traces of oil and sweat from the operator's hands on the parts. Therefore, degreasing is used to effectively clean, disperse and remove the mineral oil, lubricant and stamping and drawing oil on the surface of the parts, improve the phosphating effect and the adhesion of the electrophoretic coating, and add cleaning agent every day according to the cleaning effect, and replace all the tank liquid after 1 to 2 months;
[0011] S3, one-time water washing: wash the parts degreased in step S2 to remove the residual alkali film on the surface of the pre-treated parts, the washing time is 1 to 2 minutes, the working temperature is 50 to 60°C, and the water is replaced according to the cleaning condition of the parts;
[0012] S4. Phosphating treatment: refers to a surface chemical treatment method in which a metal surface is contacted with an acidic solution containing dihydrogen phosphate to produce a chemical reaction to form a stable, insoluble inorganic compound film (phosphating film) on the metal surface. The washed parts are placed in a phosphating bath at a bath temperature of 35-40°C for 5-6 minutes, and the total acidity and free acidity of the bath are controlled within a certain range;
[0013] S5. Secondary water washing: Use pure water to fully wash the phosphating parts to prevent the acid, alkali and salt from the previous process from being brought into the electrophoresis tank to pollute the paint tank and affect the paint film;
[0014] S6. Electrophoresis:
[0015] 1) Parts must be manually wiped before going online, and only after being wiped clean can they be put online; the filter should replace the oil removal filter bag, find out the source of oil pollution, and strictly prohibit oil pollution from entering the tank liquid; adjust the pigment-to-base ratio of the electrophoresis tank liquid, add color paste, and increase the pigment content;
[0016] 2) Place the parts in a cathode electrophoresis tank with a temperature of 28-32°C, a voltage of 170-230V, a conductivity (25°C) of 1000-1800μs / cm, a solid content of 19-21%, and a pigment-to-base ratio of 0.18-0.24 for electrophoresis for 3-4 minutes;
[0017] 3) Control the phosphorus conversion film formation time, adjust the phosphorus-free conversion related process parameters, and control the phosphorus-free conversion film thickness; immediately clean with UF liquid after the electrophoresis tank to avoid abnormal line stop; reduce the electrophoresis voltage and adjust the electrophoresis tank liquid temperature to within the process range; strengthen the tank liquid circulation stirring, control the liquid surface flow rate and the main and auxiliary tank drop, and eliminate the foam accumulated on the liquid surface;
[0018] 4) Reduce the electrophoresis voltage or tank temperature to avoid too close distance between electrodes; discharge fresh UF solution, add pure water, and control the impurity ion and solvent content in the electrophoresis tank;
[0019] 5) Strengthen cleaning after electrophoresis, increase fresh pure water spray at the outlet, etc.; reduce the paint content in the post-cleaning UF liquid, and appropriately reduce the solid content of the tank liquid; improve the structure of the coated parts, open holes for drainage, and adjust the process parameters of the water blowing device;
[0020] 6) Increase the solid content in the electrophoresis tank liquid, increase the replacement frequency of the filter bag, and accelerate the tank liquid renewal cycle; reduce the amount of color paste added and reduce the pigment-to-base ratio of the electrophoresis tank liquid; add solvent to increase the organic solvent content of the electrophoresis tank liquid; discharge fresh ultrafiltrate and add pure water to the electrophoresis tank; strengthen the circulation and stirring of the electrophoresis tank liquid, adjust the liquid surface flow rate within the process range; adjust the temperature of the electrophoresis tank liquid within the process range;
[0021] S7, ultrafiltration water washing: recycling water washing, reducing paint waste and reducing production costs, the temperature is room temperature, the time is 1 to 2 minutes;
[0022] S8. Baking: The electrophoretic paint film is cured at a temperature of 160 to 180°C for 20 to 25 minutes.
[0023] Preferably, before placing the parts to be processed in step S1, rust, metal fragments and welding slag on the surface of the parts are removed with 80-120 mesh sandpaper to eliminate potential dust sources of phosphating and electrophoresis. The degreasing time in step S2 is 5-8 minutes, the working temperature is 60-70°C, and the cleaning agent concentration is 4-5%.
[0024] Preferably, after washing the parts once in step S3, a titanium-based surface conditioner is used to adjust the surface of the parts to form a dense and uniform phosphating film, the adjustment time is 1 to 2 minutes, the working temperature is room temperature, and the concentration of the surface conditioner is 0.3 to 0.5%.
[0025] Preferably, in step S4, the total acidity and the free acidity are controlled at 14-22 points and 0.6-1.2 points respectively, and in step S5, the conductivity of pure water is less than 5 μs / cm.
[0026] Preferably, in step S8, when baking the parts, a pre-drying section is added to preheat the coated object at a temperature of 60-100° C. to prevent the accumulated liquid in the gap from rapidly heating up and boiling and flowing out.
[0027] (III) Beneficial effects
[0028] Compared with the prior art, the present invention provides an electrophoresis process for the production and processing of new energy vehicle parts, which has the following beneficial effects:
[0029] The electrophoretic process for the production and processing of new energy vehicle parts improves the electrophoretic quality of the electrophoretic paint by setting the temperature requirements for the electrophoretic paint during coating, making the temperature and electrodes of the parts moderate during electrophoresis, neutralizing the electrodeposition speed of the electrophoretic paint, making the thickness of the electrophoretic layer uniform, reducing the generation of cracks, reducing the solvent volatilization of the tank liquid, and improving the stability of the electrophoretic paint. At the same time, after understanding the causes of the electrophoretic process of automotive parts, such as shrinkage holes, pinholes, and abnormal adhesion, the right remedies are given to ensure that the electrophoretic layer can completely cover the hidden places, and has strong adhesion, is not easy to fall off, has strong corrosion resistance, is flat and smooth, and is more in line with environmental protection requirements, so that the coating quality can be stably controlled, thereby further improving the electrophoretic quality. In addition, in the entire electrophoretic process, after the manual surface treatment of the parts, a series of subsequent electrophoretic processing can be carried out, so that the electrophoretic processing efficiency of the parts is further improved. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1:
[0032] An electrophoresis process for the production and processing of new energy vehicle parts comprises the following steps:
[0033] S1. Placement: Hang the parts on a special rack, hang them firmly and securely, and polish the contact points between the rack and the parts until the metallic luster is exposed to ensure good conductivity. Before placing the parts to be processed, use 80-grit sandpaper to remove rust, metal fragments and welding slag on the surface of the parts to eliminate potential dust sources for phosphating and electrophoresis;
[0034] S2, degreasing: Since parts are usually protected with anti-rust grease during storage and transportation, there are often oil and sweat marks on the parts from the operator's hands. Therefore, degreasing is used to effectively clean, disperse and remove the mineral oil, lubricant and stamping and drawing oil on the surface of the parts, improve the phosphating effect and the adhesion of the electrophoretic coating, and add cleaning agent every day according to the cleaning effect. After 1 month, replace all the tank liquids. The degreasing time is 5 minutes, the working temperature is 60°C, and the cleaning agent concentration is 4%;
[0035] S3, one-time water washing: wash the parts after degreasing in step S2 to remove the residual alkali film on the surface of the pre-treated parts, the washing time is 1 minute, the working temperature is 50°C, and the water is changed according to the cleaning condition of the parts. After the parts are washed with water, the surface of the parts is adjusted with a titanium surface conditioner to form a sparse and uniform phosphating film, the adjustment time is 1 minute, the working temperature is room temperature, and the surface conditioner ratio concentration is 0.3%;
[0036] S4, phosphating treatment: refers to a surface chemical treatment method in which a metal surface is contacted with an acidic solution containing dihydrogen phosphate to produce a chemical reaction to form a stable, insoluble inorganic compound film (phosphating film) on the metal surface. The washed parts are placed in a phosphating bath at a bath temperature of 35°C for 5 minutes, and the total acidity and free acidity of the bath are controlled within a certain range, wherein the total acidity and free acidity are controlled at 14 points and 0.6 points respectively, and the conductivity of pure water is less than 5μs / cm;
[0037] S5. Secondary water washing: Use pure water to fully wash the phosphating parts to prevent the acid, alkali and salt from the previous process from being brought into the electrophoresis tank to pollute the paint tank and affect the paint film;
[0038] S6. Electrophoresis:
[0039] 1) Parts must be manually wiped before going online, and only after being wiped clean can they be put online; the filter should replace the oil removal filter bag, find out the source of oil pollution, and strictly prohibit oil pollution from entering the tank liquid; adjust the pigment-to-base ratio of the electrophoresis tank liquid, add color paste, and increase the pigment content;
[0040] 2) Place the parts in a cathode electrophoresis tank with a temperature of 28°C, a voltage of 170V, a conductivity (25°C) of 1000μs / cm, a solid content of 19%, and a pigment-to-base ratio of 0.18 for electrophoresis for 3 minutes;
[0041] 3) Control the phosphorus conversion film formation time, adjust the phosphorus-free conversion related process parameters, and control the phosphorus-free conversion film thickness; immediately clean with UF liquid after the electrophoresis tank to avoid abnormal line stop; reduce the electrophoresis voltage and adjust the electrophoresis tank liquid temperature to within the process range; strengthen the tank liquid circulation stirring, control the liquid surface flow rate and the main and auxiliary tank drop, and eliminate the foam accumulated on the liquid surface;
[0042] 4) Reduce the electrophoresis voltage or tank temperature to avoid too close distance between electrodes; discharge fresh UF solution, add pure water, and control the impurity ion and solvent content in the electrophoresis tank;
[0043] 5) Strengthen cleaning after electrophoresis, increase fresh pure water spray at the outlet, etc.; reduce the paint content in the post-cleaning UF liquid, and appropriately reduce the solid content of the tank liquid; improve the structure of the coated parts, open holes for drainage, and adjust the process parameters of the water blowing device;
[0044] 6) Increase the solid content in the electrophoresis tank liquid, increase the replacement frequency of the filter bag, and accelerate the tank liquid renewal cycle; reduce the amount of color paste added and reduce the pigment-to-base ratio of the electrophoresis tank liquid; add solvent to increase the organic solvent content of the electrophoresis tank liquid; discharge fresh ultrafiltrate and add pure water to the electrophoresis tank; strengthen the circulation and stirring of the electrophoresis tank liquid, adjust the liquid surface flow rate within the process range; adjust the temperature of the electrophoresis tank liquid within the process range;
[0045] S7, ultrafiltration water washing: recycling water washing, reducing paint waste and reducing production costs, the temperature is room temperature, the time is 1 minute;
[0046] S8, baking: the electrophoretic paint film is cured at a temperature of 160°C for 20 minutes. When baking parts, a pre-drying section needs to be added, and the coated object is preheated at 60°C to prevent the accumulated liquid in the gap from boiling rapidly and flowing out.
[0047] Embodiment 2:
[0048] An electrophoresis process for the production and processing of new energy vehicle parts comprises the following steps:
[0049] S1. Placement: Hang the parts on a special rack, hang them firmly and securely, and polish the contact points between the rack and the parts until the metallic luster is exposed to ensure good conductivity. Before placing the parts to be processed, use 120-grit sandpaper to remove rust, metal fragments and welding slag on the surface of the parts to eliminate potential dust sources of phosphating and electrophoresis;
[0050] S2, degreasing: Since parts are usually protected with anti-rust grease during storage and transportation, there are often oil and sweat marks on the parts from the operator's hands. Therefore, degreasing is used to effectively clean, disperse and remove the mineral oil, lubricant and stamping and drawing oil on the surface of the parts, improve the phosphating effect and the adhesion of the electrophoretic coating, and add cleaning agent every day according to the cleaning effect. Replace all tank liquids after 2 months. The degreasing time is 8 minutes, the working temperature is 70°C, and the cleaning agent concentration is 5%;
[0051] S3, one-time water washing: wash the parts after degreasing in step S2 to remove the residual alkali film on the surface of the pre-treated parts, the washing time is 2 minutes, the working temperature is 60°C, and the water liquid is changed according to the cleaning condition of the parts. After the parts are washed with water, the surface of the parts is adjusted with a titanium surface conditioner to form a sparse and uniform phosphating film, the adjustment time is 2 minutes, the working temperature is room temperature, and the surface conditioner ratio concentration is 0.5%;
[0052] S4, phosphating treatment: refers to a surface chemical treatment method in which a metal surface is contacted with an acidic solution containing dihydrogen phosphate to produce a chemical reaction to form a stable, insoluble inorganic compound film (phosphating film) on the metal surface. The washed parts are placed in a phosphating bath at a bath temperature of 40°C for 6 minutes, and the total acidity and free acidity of the bath are controlled within a certain range, wherein the total acidity and free acidity are controlled at 22 points and 1.2 points respectively, and the conductivity of pure water is less than 5μs / cm;
[0053] S5. Secondary water washing: Use pure water to fully wash the phosphating parts to prevent the acid, alkali and salt from the previous process from being brought into the electrophoresis tank to contaminate the paint tank and affect the paint film;
[0054] S6. Electrophoresis:
[0055] 1) Parts must be manually wiped before going online, and only after being wiped clean can they be put online; the filter should replace the oil removal filter bag, find out the source of oil pollution, and strictly prohibit oil pollution from entering the tank liquid; adjust the pigment-to-base ratio of the electrophoresis tank liquid, add color paste, and increase the pigment content;
[0056] 2) Place the parts in a cathode electrophoresis tank with a temperature of 32°C, a voltage of 230V, a conductivity (25°C) of 1800μs / cm, a solid content of 21%, and a pigment-to-base ratio of 0.24 for electrophoresis for 4 minutes;
[0057] 3) Control the phosphorus conversion film formation time, adjust the phosphorus-free conversion related process parameters, and control the phosphorus-free conversion film thickness; immediately clean with UF liquid after the electrophoresis tank to avoid abnormal line stop; reduce the electrophoresis voltage and adjust the electrophoresis tank liquid temperature to within the process range; strengthen the tank liquid circulation stirring, control the liquid surface flow rate and the main and auxiliary tank drop, and eliminate the foam accumulated on the liquid surface;
[0058] 4) Reduce the electrophoresis voltage or tank temperature to avoid too close distance between electrodes; discharge fresh UF solution, add pure water, and control the impurity ion and solvent content in the electrophoresis tank;
[0059] 5) Strengthen cleaning after electrophoresis, increase fresh pure water spray at the outlet, etc.; reduce the paint content in the post-cleaning UF liquid, and appropriately reduce the solid content of the tank liquid; improve the structure of the coated parts, open holes for drainage, and adjust the process parameters of the water blowing device;
[0060] 6) Increase the solid content in the electrophoresis tank liquid, increase the replacement frequency of the filter bag, and accelerate the tank liquid renewal cycle; reduce the amount of color paste added and reduce the pigment-to-base ratio of the electrophoresis tank liquid; add solvent to increase the organic solvent content of the electrophoresis tank liquid; discharge fresh ultrafiltrate and add pure water to the electrophoresis tank; strengthen the circulation and stirring of the electrophoresis tank liquid, adjust the liquid surface flow rate within the process range; adjust the temperature of the electrophoresis tank liquid within the process range;
[0061] S7, ultrafiltration water washing: recycling water washing, reducing paint waste and reducing production costs, the temperature is room temperature, the time is 2 minutes;
[0062] S8, baking: the electrophoretic paint film is cured at a temperature of 180°C for 25 minutes. When baking parts, a pre-drying section needs to be added, and the coated object is preheated at 100°C to prevent the accumulated liquid in the gap from boiling rapidly and flowing out.
[0063] The beneficial effects of the present invention are: by strictly controlling the electrophoretic temperature of the electrophoretic paint during coating, the temperature of the parts and the electrodes are moderate during electrophoresis, that is, the cathode electrophoretic bath liquid temperature is 28-32°C, the pH value and the conductivity are controlled at 5.8-6.4 and 1000-1800 μs / cm respectively to maintain the stability of the bath liquid and the coating quality, the electrophoretic deposition rate of the electrophoretic paint is neutralized, the thickness of the electrophoretic layer is uniform, the generation of cracks is reduced, and the solvent volatilization of the bath liquid is reduced, and the stability of the electrophoretic paint is improved, so as to improve the electrophoretic quality of the electrophoretic paint. At the same time, we understand the reasons why automobile parts are produced during the electrophoresis process, such as shrinkage holes, pinholes, and abnormal adhesion, and then prescribe the right remedies to ensure that the electrophoretic layer can completely cover the hidden places, and has strong adhesion, is not easy to fall off, has strong corrosion resistance, is flat and smooth, and is more in line with environmental protection requirements, so that the coating quality can be stably controlled, thereby further improving the quality of electrophoresis. In the entire electrophoresis process, after the surface of the parts is manually treated, a series of subsequent electrophoresis processing can be carried out to further improve the electrophoresis processing efficiency of the parts.
[0064] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An electrophoresis process for the production and processing of new energy vehicle parts. It is characterized in that The following steps are involved: S1. Placement: Hang the parts on a special rack, hang them firmly and securely, and polish the contact points between the rack and the parts until the metallic luster is exposed to ensure good conductivity; S2. Degreasing: As parts are usually protected with anti-rust grease during storage and transportation, there are often traces of oil and sweat from the operator's hands on the parts. Therefore, degreasing is used to effectively clean, disperse and remove the mineral oil, lubricant and stamping and drawing oil on the surface of the parts, improve the phosphating effect and the adhesion of the electrophoretic coating, and add cleaning agent every day according to the cleaning effect, and replace all the tank liquid after 1 to 2 months; S3, one-time water washing: wash the parts degreased in step S2 to remove the residual alkali film on the surface of the pre-treated parts, the washing time is 1 to 2 minutes, the working temperature is 50 to 60°C, and the water is replaced according to the cleaning condition of the parts; S4. Phosphating treatment: refers to a surface chemical treatment method in which a metal surface is contacted with an acidic solution containing dihydrogen phosphate to produce a chemical reaction to form a stable, insoluble inorganic compound film (phosphating film) on the metal surface. The washed parts are placed in a phosphating bath at a bath temperature of 35-40°C for 5-6 minutes, and the total acidity and free acidity of the bath are controlled within a certain range; S5. Secondary water washing: Use pure water to fully wash the phosphating parts to prevent the acid, alkali and salt from the previous process from being brought into the electrophoresis tank to pollute the paint tank and affect the paint film; S6. Electrophoresis: 1) Parts need to be wiped manually before going online, and then put online after being wiped clean; Replace the oil removal filter bag of the filter, find out the source of oil pollution, and strictly prohibit oil pollution from entering the tank liquid; adjust the pigment-base ratio of the electrophoresis tank liquid, add color paste, and increase the pigment content; 2) Place the parts in a cathode electrophoresis tank with a temperature of 28-32°C, a voltage of 170-230V, a conductivity (25°C) of 1000-1800μs / cm, a solid content of 19-21%, and a pigment-to-base ratio of 0.18-0.24 for electrophoresis for 3-4 minutes; 3) Control the phosphorus conversion film forming time, adjust the phosphorus-free conversion related process parameters, and control the phosphorus-free conversion film thickness; immediately clean with UF liquid after electrophoresis out of the tank to avoid abnormal line stop; Reduce the electrophoresis voltage and adjust the electrophoresis tank liquid temperature to within the process range; strengthen the tank liquid circulation stirring, control the liquid surface flow rate and the main and auxiliary tank drop, and eliminate the foam accumulated on the liquid surface; 4) Reduce the electrophoresis voltage or tank temperature to avoid too close distance between electrodes; discharge fresh UF solution, add pure water, and control the impurity ion and solvent content in the electrophoresis tank; 5) Strengthen cleaning after electrophoresis, increase fresh pure water spray at the outlet, etc.; reduce the paint content in the post-cleaning UF liquid, and appropriately reduce the solid content of the tank liquid; improve the structure of the coated parts, open holes for drainage, and adjust the process parameters of the water blowing device; 6) Increase the solid content in the electrophoresis tank liquid, increase the replacement frequency of the filter bag, and accelerate the tank liquid renewal cycle; reduce the amount of color paste added and reduce the pigment-to-base ratio of the electrophoresis tank liquid; add solvent to increase the organic solvent content of the electrophoresis tank liquid; discharge fresh ultrafiltrate and add pure water to the electrophoresis tank; strengthen the circulation and stirring of the electrophoresis tank liquid, adjust the liquid surface flow rate within the process range; adjust the temperature of the electrophoresis tank liquid within the process range; S7, ultrafiltration water washing: recycling water washing, reducing paint waste and reducing production costs, the temperature is room temperature, the time is 1 to 2 minutes; S8. Baking: The electrophoretic paint film is cured at a temperature of 160 to 180°C for 20 to 25 minutes.
2. The electrophoresis process for producing and processing new energy vehicle parts according to claim 1, It is characterized in that Before placing the parts to be processed in step S1, rust, metal fragments and welding slag on the surface of the parts need to be removed with 80-120 mesh sandpaper to eliminate potential dust sources of phosphating and electrophoresis. The degreasing time in step S2 is 5-8 minutes, the working temperature is 60-70° C., and the cleaning agent concentration is 4-5%.
3. The electrophoresis process for producing and processing new energy vehicle parts according to claim 1, It is characterized in that After washing the parts once in step S3, titanium-based surface conditioner is used to condition the surface of the parts to form a dense and uniform phosphating film. The conditioning time is 1 to 2 minutes, the working temperature is room temperature, and the surface conditioner concentration is 0.3 to 0.5%.
4. The electrophoresis process for producing and processing new energy vehicle parts according to claim 1, It is characterized in that In the step S4, the total acidity and the free acidity are controlled at 14-22 points and 0.6-1.2 points respectively, and in the step S5, the conductivity of the pure water is less than 5 μs / cm.
5. The electrophoresis process for producing and processing new energy vehicle parts according to claim 1, It is characterized in that When baking the parts in step S8, a pre-drying section needs to be added to preheat the coated object at a temperature of 60-100° C. to prevent the accumulated liquid in the gap from rapidly heating up and boiling and flowing out.