Macroscopic-size LaOCl single crystal as well as preparation method and application thereof
By using the self-flux method or external flux method to grow LaOCl single crystals in high-temperature vacuum or air environment during the preparation process of LaOCl, the problem of the size limitation of LaOCl single crystals in the prior art is solved, and the preparation of centimeter-level single crystals is realized and The peeling of large-area nanosheets meets the application needs of two-dimensional Highκ dielectrics.
Patent Information
- Application Number
- CN202411070810.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-29
AI Technical Summary
The existing LaOCl preparation method is difficult to grow single crystals of macroscopic size, and is limited to the micron level, which cannot meet the application needs of two-dimensional Highκ dielectrics.
The self-flux method or external flux method is used to grow LaOCl single crystals in a vacuum or air environment through high temperature reaction. The excessive LaCl3 and external flux KCl are used to provide a suitable molten salt environment, and the sintering temperature is increased to 920-1050℃ to ensure the precursor. After sufficient reaction, a single crystal of LaOCl at the centimeter scale was obtained.
The macroscopic LaOCl single crystal was successfully prepared, breaking through the micron-scale limitation, and able to peel off large areas into high-quality LaOCl nanosheets. It is suitable for two-dimensional Highκ dielectrics and provides a broader application prospect.
Smart Images

Figure CN119041002A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of dielectric materials, and in particular to a macroscopic LaOCl single crystal and a preparation method and application thereof. Background Art
[0002] Lanthanum oxychloride (LaOCl) has a tetragonal structure, a space group of P4 / nmm, and a lattice parameter of Due to the advantages of LaOCl such as high dielectric constant, wide bandgap, high breakdown field strength, and strong stability in air, LaOCl has potential important application value in future microelectronic insulation layers, electronic packaging layers, and gate dielectrics in two-dimensional field effect transistors.
[0003] However, in existing research, the preparation of rare earth oxyhalide LaOCl mainly relies on electrospinning, molten salt method and sol-gel method. In 2010, document 1 recorded that Li et al. prepared LaOCl nanofibers by electrospinning, however, the diameter of the fiber was generally only 300-400nm. In 2017, document 2 recorded that Huang et al. prepared single-crystalline LaOCl nanosheets by molten salt method, however, the size of the nanosheets was only 5-20μm. In 2019, document 3 recorded that Zhu et al. prepared LaOCl samples by sol-gel method, but the samples were polycrystalline powders. In 2023, documents 4 and 5 recorded that Zhang, Dang et al. grew small single-crystalline nanosheets with uniform thickness by molten salt method, chemical vapor deposition (CVD) and other methods, respectively, however, the size of the nanosheets was still limited to the micrometer level. The application of two-dimensional Highκ dielectrics requires that the dielectrics are large-sized uniform nanosheets. Directly peeling off high-quality large-area nanosheets from single crystals is a potential application method. Therefore, developing methods for growing macroscopic single-crystalline LaOCl and corresponding crystal growth methods is very important for the application of LaOCl in the future microelectronics field.
[0004] References:
[0005] Literature 1: Li G, Hou Z, Peng C, et al. Electrospinning Derived One-DimensionalLaOCl:Ln 3+ (Ln=Eu / Sm,Tb,Tm)Nanofibers, Nanotubes and Microbelts withMulticolor-Tunable Emission Properties[J]. Advanced Functional Materials, 2010, 20: 3446-3456;
[0006] Document 2: Huang Z., Zhang HJ, Zhang XW, Growth of well-developed LaOClmicroplates by chloride salt-assisted method[J].Crystengcomm 2017,19:2971-2976
[0007] Document 3: Zhu XR, Hope-Weeks LJ, Ramirez D., etal. Controlabledecomposition of lanthanum oxychloride through different annealing conditions [J]. Journal of Alloys and Compounds 2019,800:29-34
[0008] Document 4: Zhang B, Zhu YC, Zhao ZJ, et al. General Approach for Two-Dimensional Rare-Earth Oxyhalides with High Gate Dielectric Performance[J]. Journal of the American Chemical Society.2023,145,20:11074–11084
[0009] Document 5: Li L, Dang W, Zhu Summary of the invention
[0010] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a macro-sized LaOCl single crystal and a preparation method and application thereof.
[0011] The purpose of the present invention can be achieved by the following technical solutions:
[0012] One of the technical solutions of the present invention is to provide a method for preparing a macroscopic LaOCl single crystal, including a self-flux method or an external flux method;
[0013] The self-fluxing method comprises the following steps: 2 O 3 ) powder and lanthanum chloride (LaCl 3 ) powders to obtain a precursor, react at high temperature under a vacuum environment, and after the reaction is completed, cool, clean, and separate to obtain a LaOCl single crystal;
[0014] The external flux method steps are: La 2 O 3 Powder and LaCl 3 The powders are mixed to obtain a precursor, an external flux is added to the precursor, a high-temperature reaction is performed, and after the reaction is completed, the temperature is lowered, the precursor is cleaned, and the LaOCl single crystal is obtained by separation.
[0015] Furthermore, in the self-fluxing method, the LaCl 3 Powder and La 2 O 3 The minimum mass ratio of powder is (5-20):1.
[0016] Furthermore, in the self-fluxing method, the temperature of the high temperature reaction is 920-970° C., and the time is 12-72 hours, specifically 12 hours, 24 hours, 48 hours, 60 hours, or 72 hours.
[0017] Furthermore, in the self-flux method, the apparatus for high-temperature reaction is a tubular furnace.
[0018] Furthermore, in the external flux method, the external flux is potassium chloride (KCl) powder.
[0019] Furthermore, in the external flux method, the La 2 O 3 Powder and LaCl 3 The mass ratio of powder is (5-20):1; external flux and LaCl 3 The mass ratio of the powder is (4-20):1.
[0020] Furthermore, in the external flux method, the temperature of the high temperature reaction is 970-1050° C., the time is 12-72 hours, specifically 12 hours, 24 hours, 48 hours, 60 hours, 72 hours, and the environment is a vacuum environment or an air environment.
[0021] Furthermore, in the external flux method, the apparatus for the high temperature reaction is a tube furnace or a box furnace (muffle furnace).
[0022] Furthermore, in the self-flux method and the external flux method, the cleaning solution used for cleaning is deionized water and dilute hydrochloric acid. The deionized water is used to clean the sample, and the dilute hydrochloric acid is used to remove the residual La 2 O3 .
[0023] Furthermore, the concentration of the dilute hydrochloric acid is 0.5-4 mol / L.
[0024] The second technical solution of the present invention is to provide a macroscopic LaOCl single crystal, which is prepared by the above-mentioned preparation method.
[0025] Furthermore, the band gap value of the LaOCl single crystal is about 5 to 6 eV.
[0026] The third technical solution of the present invention is to provide an application of a macroscopic LaOCl single crystal in the field of dielectric materials, which is used as a packaging layer or a gate dielectric layer to prepare field effect transistors and logic devices.
[0027] Furthermore, the LaOCl single crystal is mechanically exfoliated to obtain LaOCl nanosheets, and the LaOCl single crystal is mechanically exfoliated with a tape and then attached to a Si substrate or Si / SiO 2 Carried out on the base.
[0028] Furthermore, the tape is a fiber tape, the tape can be attached and separated 4 to 8 times, the low temperature treatment temperature when attached to the Si substrate is -10 to -20°C, and the tape and the silicon (Si) substrate are directly separated at low temperature.
[0029] Furthermore, the silicon / silicon oxide (Si / SiO 2 ) The substrate is 100~500nm Si / SiO 2 Substrate, the Si / SiO 2 The substrate is peeled off at room temperature.
[0030] Furthermore, the breakdown field strength of the exfoliated LaOCl nanosheet with a thickness of 20 nm is at least 9 MV / cm, preferably 9 to 12 MV / cm.
[0031] Furthermore, the exfoliation thickness of the LaOCl nanosheet is 5 to 20 nm. When the thickness of the exfoliated LaOCl nanosheet decreases, its breakdown field strength may increase with the decrease in thickness (Li W, Zhou J, Cai S, Yu Z, Zhang J, Fang N, et al. Uniform and ultrathin high-κgate dielectrics for two-dimensional electronic devices. Nature Electronics. 2019, 2 (12): 563-71). However, when the oxygen vacancy concentration in the nanosheet increases, its breakdown field strength may decrease due to the leakage conduction that may be caused by oxygen vacancies.
[0032] Compared with the prior art, the present invention has the following innovative features:
[0033] (1) The present invention introduces vacuum conditions into the self-fluxing method, raises the high-temperature sintering temperature to above 900 degrees (920-970 degrees C) for the first time, and adds an excess of LaCl 3 , so that the precursor can fully react, the excess LaCl 3 It can provide a suitable high-temperature molten salt environment for the growth of crystals throughout the entire process of high-temperature reaction, and the high vacuum environment avoids the interference of oxygen and moisture in the air on the sample.
[0034] (2) In the external flux method of the present invention, by adding an excessive amount of external flux KCl and continuing to increase the high-temperature sintering temperature to (970-1050° C.), the high-temperature reaction can be carried out in an air environment, thereby expanding the scope of the reaction.
[0035] (3) The present invention prepares macroscopic (centimeter-level) LaOCl single crystals by self-fluxing method and external flux method, breaking through the limitation of micron-level, and can be used in two-dimensional Highκ dielectrics. The present invention provides two methods for preparing macroscopic LaOCl single crystals. The two methods are simple and easy to operate, with good repeatability. The obtained LaOCl single crystal blocks are easily peeled off into large-area LaOCl nanosheets, which have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a macroscopic crystal optical image of the LaOCl single crystal bulk shown in Example 1;
[0037] Figure 2 This is a macroscopic crystal optical image of the LaOCl single crystal bulk shown in Example 2;
[0038] Figure 3 X-ray diffraction data of the LaOCl single crystal bulk shown in Example 1 and Example 2;
[0039] Figure 4 High-resolution electron microscopy (AC-HRTEM) data of the LaOCl single crystal shown in Example 1;
[0040] Figure 5 High-resolution electron microscopy (AC-HRTEM) data of the LaOCl single crystal shown in Example 2;
[0041] Figure 6 is the selected area electron diffraction (SAED) pattern of the LaOCl single crystal shown in Example 1;
[0042] Figure 7The selected area electron diffraction (SAED) pattern of the LaOCl single crystal shown in Example 2; The optical image of the LaOCl nanosheet shown;
[0043] Figure 8 The UV-visible absorption spectrum and band gap of the LaOCl single crystal bulk shown in Example 1;
[0044] Fig. 9 This is an optical image of the LaOCl nanosheets shown in Example 3;
[0045] Fig.10 The atomic force microscope images corresponding to the LaOCl nanosheets shown in Example 3, (a) AFM image of the nanosheets, (b) the corresponding thickness data extracted from the white line in Figure a;
[0046] Fig.11 IV curve of the 20 nm thick LaOCl nanosheet peeled off as shown in Example 3, (a) MIM structure prepared by nanosheet, (b) IV data showing a breakdown field strength of 9 MV / cm, (c) AFM image of the nanosheet edge, (d) thickness data extracted from Figure c.
[0047] Fig.12 Optical image of LaOCl sample prepared by self-fluxing method in air atmosphere;
[0048] Fig.13 XRD diffraction pattern of LaOCl sample prepared by self-fluxing method in air atmosphere;
[0049] Fig.14 Optical image of LaOCl sample prepared with NaCl as external solvent;
[0050] Fig.15 This is the XRD diffraction pattern of LaOCl sample prepared with NaCl as external solvent. DETAILED DESCRIPTION
[0051] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments. Based on the given embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0052] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. The following are the models and sources of some reagents and experimental materials.
[0053] In the following examples, LaCl 3The CAS number is 10099-58-8, La 2 O 3 The CAS number of the reagent is 1312-81-8, purchased from Shanghai Adamas Reagent Co., Ltd.; the model of the 3M tape is US version 600, purchased from 3M Company of the United States; the purity of the Si wafer is ≥99.9999%, Si / SiO 2 It has a 300nm oxide layer and was purchased from Guangzhou Fangdao Semiconductor Co., Ltd.
[0054] Example 1
[0055] The preparation process of macro-sized LaOCl single crystals by the self-flux method is as follows:
[0056] Weigh 1g La 2 O 3 (99.99%) and 10 g LaCl 3 (99.99%), mix them evenly, pour them into a corundum crucible and place them in a high vacuum (10 -4 Torr) quartz tube, the outer diameter of the quartz tube is 80mm and the length is 100cm. The central heating zone of the tube furnace is heated to 950℃, the heating rate is 5℃ / min, and the temperature is kept for 12 hours to grow LaOCl single crystal. After the growth is completed, the furnace is cooled to 200℃ at a rate of 150℃ / h, and finally cooled naturally to room temperature. The above sample is washed with deionized water and 1mol / L dilute hydrochloric acid to obtain LaOCl single crystal block.
[0057] like Figure 1 As shown, the size of the LaOCl single crystal block prepared by the self-flux method is close to 1 cm when measured under macroscopic conditions.
[0058] Example 2
[0059] The external flux method is used to prepare macroscopic LaOCl single crystals. The preparation process is as follows:
[0060] Weigh 0.5 g La 2 O 3 (99.99%) and 5g LaCl 3 (99.99%) and mix them evenly to obtain a precursor. Pour it into a corundum crucible with 10g KCl on the bottom, and then cover the precursor with 50g KCl. Place the corundum crucible with the precursor in the central heating zone of a box furnace or a tube furnace, heat it to 1000°C at a rate of 5°C / min, and keep it warm for 24 hours to grow LaOCl single crystals. After the growth is completed, cool the furnace to 200°C at a rate of 150°C / h, and finally cool it naturally to room temperature. Wash the above sample with deionized water and 4mol / L dilute hydrochloric acid to obtain a LaOCl single crystal block.
[0061] like Figure 2 As shown, the size of the LaOCl single crystal block prepared by the external flux method is greater than 1 cm when measured under macroscopic conditions.
[0062] like Figure 3 As shown, X-ray diffraction analysis was performed on the LaOCl single crystal blocks prepared in Example 1 and Example 2. The XRD data of the LaOCl samples prepared by the two preparation methods showed a strong and sharp (00h) peak, indicating the high-quality single crystal nature of the samples.
[0063] The high resolution electron microscopy (AC-HRTEM) data of the LaOCl samples prepared in Examples 1 and 2 are as follows: Figure 4 and Figure 5 As shown, the samples from both methods showed a tetragonal structure, and the interplanar spacing with an interface angle of 90 degrees was measured to be 0.288nm and 0.287nm, which is consistent with the crystal structure of LaOCl.
[0064] The selected area electron diffraction (SAED) patterns of the LaOCl single crystal bulk obtained in Examples 1 and 2 are as follows: Figure 6 and Figure 7 As shown, a group of sharp diffraction spots appeared in the image, verifying that LaOCl has single crystal properties and four-fold symmetry.
[0065] Figure 8 The UV-visible absorption spectrum and band gap of the LaOCl single crystal bulk prepared in Example 1. The band gap can be calculated from the UV-visible absorption spectrum of the LaOCl single crystal. The results are as follows: Figure 8 As shown, the band gap value of LaOCl is about 5.3 eV.
[0066] Example 3
[0067] The preparation process of LaOCl nanosheets is as follows:
[0068] A section of 3M tape was pasted on the LaOCl single crystal block prepared in Example 1, and then the tape was folded in half 4 times to ensure that the LaOCl single crystal block was evenly distributed on the tape. Next, a clean silicon wafer was aligned with the portion of the tape with the LaOCl single crystal block, and gently pressed to form a good bond between the LaOCl single crystal block and the silicon wafer, and the bonded silicon wafer was placed in a -18°C freezer for low temperature treatment for 12 hours, and then directly torn off at low temperature to obtain LaOCl nanosheets.
[0069] The peeled silicon wafer is placed under a microscope for observation to find the desired LaOCl nanosheets.
[0070] Fig. 9This is the thinnest LaOCl nanosheet peeled off in Example 3. The nanosheet appears brown on the silicon wafer. The color of the nanosheet can distinguish the thickness of the nanosheet, and the thinner area appears more transparent.
[0071] Fig.10 This is the atomic force microscope image corresponding to the LaOCl nanosheet of Example 3. The AFM data shows that the thickness of the thinnest area of the nanosheet is 10 nm.
[0072] Example 4
[0073] The preparation process of LaOCl nanosheets is as follows:
[0074] A piece of 3M fiber tape was pasted on the LaOCl single crystal block prepared in Example 2, and then the tape was folded in half 8 times to ensure that the LaOCl single crystal block was evenly distributed on the tape. 2 The substrate is aligned with the part of the tape where the LaOCl single crystal block is located, and gently pressed to make the LaOCl single crystal block and Si / SiO 2 The substrates form good adhesion and the Si / SiO 2 The substrate was placed in a -18°C freezer for low-temperature treatment for 12 hours and then torn off at room temperature to obtain LaOCl nanosheets.
[0075] The peeled Si / SiO 2 The substrate was placed under a microscope and observed to find the desired LaOCl nanosheets.
[0076] Fig.11 The IV curve of the 20 nm thick LaOCl nanosheet peeled off in Example 3. The IV data show that: the 20 nm thick LaOCl nanosheet ( Fig.11 aThe breakdown field strength of the red box is as high as 9MV / cm.
[0077] Example 5
[0078] Compared with Example 1, most of the above are the same, except that 1 g of La 2 O 3 (99.99%) and 5g LaCl 3 (99.99%).
[0079] Example 6
[0080] Compared with Example 1, most of the above are the same, except that 1 g of La 2 O 3 (99.99%) and 20g LaCl 3 (99.99%).
[0081] Example 7
[0082] Compared with Example 1, most of the processes are the same except that the central heating zone of the tube furnace is heated to 970°C.
[0083] Example 8
[0084] Compared with Example 1, most of the processes are the same except that the central heating zone of the tube furnace is heated to 920°C.
[0085] Example 9
[0086] Compared with Example 2, most of the above are the same, except that 1 g of La 2 O 3 (99.99%) and 5g LaCl 3 (99.99%) and mix them evenly to obtain a precursor, which is poured into a corundum crucible with 5g of KCl on the bottom, and then covered with 25g of KCl.
[0087] Example 10
[0088] Compared with Example 2, most of the above are the same, except that 1 g of La 2 O 3 (99.99%) and 20g LaCl 3 (99.99%) and mix them evenly to obtain a precursor, which is poured into a corundum crucible with 20g KCl on the bottom, and then covered with 100g KCl.
[0089] Embodiment 11
[0090] Compared with Example 2, most of the above are the same, except that 0.5 g La 2 O 3 (99.99%) and 5g LaCl 3 (99.99%) and mixed them evenly to obtain a precursor, which was poured into a corundum crucible with 4g KCl on the bottom, and then covered with 16g KCl.
[0091] Example 12
[0092] Compared with Example 2, most of the above are the same, except that 0.5 g La 2 O 3 (99.99%) and 5g LaCl 3 (99.99%) and mix them evenly to obtain a precursor, which is poured into a corundum crucible with 20g KCl on the bottom, and then covered with 80g KCl.
[0093] Embodiment 13
[0094] Compared with Example 2, most of the steps are the same, except that the corundum crucible with the precursor is placed in the central heating zone of a box furnace or a tube furnace and heated to 970° C. at a rate of 5° C. / min.
[0095] Embodiment 14
[0096] Compared with Example 2, most of the steps are the same, except that the corundum crucible with the precursor is placed in the central heating zone of a box furnace or a tube furnace and heated to 1050° C. at a rate of 5° C. / min.
[0097] Comparative Example 1
[0098] Compared with Example 1, most of the above are the same, except that the high temperature reaction is carried out under atmospheric conditions. Fig.12 and Fig.13 As shown in Figure 2, the crystal size of the LaOCl sample prepared in the atmosphere is still at the micrometer level, and the sample contains polycrystalline samples, which is different from Fig.13 The XRD diffraction pattern is consistent with that in .
[0099] Comparative Example 2
[0100] Compared with Example 2, most of them are the same, except that the external solvent KCl is adjusted to NaCl, such as Fig.14 As shown in Figure 2, the maximum crystal size of the LaOCl sample grown with NaCl as the external solvent is about 150 μm, and the corresponding XRD pattern is shown in Figure 2. Fig.15 As shown, the sample is pure phase and does not contain other impurities.
[0101] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing a macroscopic LaOCl single crystal, comprising a self-flux method or an external flux method; The self-fluxing method comprises the following steps: mixing La2O3 and LaCl3 powder as a precursor, using LaCl3 powder as a self-fluxing agent, adding the self-fluxing agent to the precursor, reacting at high temperature under a vacuum environment to obtain a product, and cooling, cleaning, and separating to obtain a LaOCl single crystal; The steps of the external flux method are: mixing La2O3 and LaCl3 powders as a precursor, using KCl powder as a self-flux, adding an external flux to the precursor, reacting at high temperature in air to obtain a product, and then cooling, cleaning, and separating to obtain a LaOCl single crystal.
2. The method for preparing a macroscopic LaOCl single crystal according to claim 1, characterized in that: In the self-fluxing method, the minimum mass ratio of the LaCl3 powder to the La2O3 powder is (5-20):
1.
3. The method for preparing a macroscopic LaOCl single crystal according to claim 1, characterized in that: In the self-fluxing method, the temperature of the high-temperature reaction is 920-970° C. and the time is 12-72 hours.
4. The method for preparing a macroscopic LaOCl single crystal according to claim 1, characterized in that: In the external flux method, the external flux is KCl powder.
5. The method for preparing a macroscopic LaOCl single crystal according to claim 1, characterized in that: In the external flux method, the minimum mass ratio of the LaCl3 powder to the La2O3 powder is (5-20):1; the mass ratio of the external flux to the LaCl3 powder is (4-20):
1.
6. The method for preparing a macroscopic LaOCl single crystal according to claim 1, characterized in that: In the external flux method, the temperature of the high temperature reaction is 970-1050° C., the time is 24-72 hours, and the environment is a vacuum environment or an air environment.
7. The method for preparing a macroscopic LaOCl single crystal according to claim 1, characterized in that: In the self-flux method and the external flux method, the cleaning liquid used for cleaning is deionized water and dilute hydrochloric acid.
8. A macroscopic LaOCl single crystal, prepared by the preparation method according to any one of claims 1 to 7.
9. Application of the macroscopic LaOCl single crystal as claimed in claim 8 in the field of dielectric materials, as a packaging layer or a gate dielectric layer to prepare field effect transistors and logic devices.
10. The use of a macroscopic LaOCl single crystal according to claim 9, characterized in that: The LaOCl single crystal is mechanically exfoliated to obtain LaOCl nanosheets, and the LaOCl single crystal is mechanically exfoliated with an adhesive tape and then attached to a Si substrate or a Si / SiO2 substrate.