Steel cylinder for containing electronic gas and treatment method thereof

By cleaning and circulating the inner surface of the cylinder through multiple steps to form a protective film, the impurity pollution problem in the cylinder is solved, the high purity and clarity of electronic gases are ensured, the process is simplified and the cost is reduced.

CN119042512APending Publication Date: 2024-11-29SHANGHAI SIMGUI TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410941345.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing cylinder treatment methods lead to impurities in the cylinder, which affects the purity and clarity of the electronic gas, and thus affects the smooth implementation of the semiconductor process.

Method used

By mechanically polishing, chemical cleaning, electrochemical polishing and multiple cycles of vacuuming and inert gas replacement, a protective film is formed to isolate the electronic gas from the inner surface of the cylinder to avoid contamination and chemical reactions.

Benefits of technology

It ensures high purity and clarity of electronic gases in the cylinder, simplifies the process flow, reduces costs, and avoids damage and contamination of the cylinder by heat treatment and ion implantation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119042512A_ABST
    Figure CN119042512A_ABST
Patent Text Reader

Abstract

The invention relates to a steel cylinder for containing electronic gas and a treatment method of the steel cylinder. The treatment method of the steel cylinder for containing the electronic gas comprises the following steps: forming the steel cylinder, wherein the steel cylinder comprises an inner surface and an outer surface; cleaning the inner surface of the steel cylinder; filling to-be-contained electronic gas into the steel cylinder, and standing the steel cylinder for a first preset time; and emptying the to-be-contained electronic gas in the steel cylinder, and circulating for multiple times according to preset time. According to the invention, the purity and cleanliness of the electronic gas contained in the steel cylinder are ensured, the operation is simple, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of integrated circuit manufacturing, and in particular to a steel cylinder for containing electronic gas and a processing method thereof. Background Art

[0002] Electronic special gases (hereinafter referred to as "electronic special gases") are widely used in the semiconductor and microelectronics industries. Electronic special gases mainly include hydride gases, fluoride gases, fluoroalkane gases, chloride gases, metal organic compound gases, etc. They are important and indispensable materials in the production process of electronic industries such as ultra-large-scale integrated circuits, flat panel displays, compound semiconductor devices, solar cells, optical fibers, etc. They are widely used in thin film manufacturing, etching, doping, vapor deposition, diffusion and other processes in the production process of integrated circuits and display panels.

[0003] The quality of electronic special gases mainly depends on their purity and cleanliness. Generally speaking, the purity requirement for electronic special gases reaches 5N-6N (N refers to the number of 9s in the purity percentage, for example, 5.7N means 99.9997%, and 6N means 99.9999%). At the same time, it is also required to purify the metal impurities in the electronic special gases to 10-9 to 10-12 levels. Every increase in purity by one N, and every order of magnitude decrease in the concentration of particles and metal impurities, will bring about a significant increase in process complexity and difficulty. Once the purity or cleanliness of electronic special gases does not meet the standards, the quality of downstream products will not pass the test at the least, and the entire product line will be spread and polluted at the worst, causing all products to be scrapped. Electronic gases have high requirements for gas purity. In order to facilitate storage and transportation, steel cylinders have become an important carrier in the production, transportation, storage and use of electronic gases. However, the quality of the steel cylinder processing method directly affects the purity and cleanliness of the electronic gas contained in the steel cylinder. However, the current steel cylinder processing method leaves impurities in the treated steel cylinder, which can easily pollute the electronic gas contained in the steel cylinder and affect the smooth implementation of subsequent semiconductor processes.

[0004] Therefore, how to optimize the processing technology of steel cylinders used to contain electronic gases, so as to ensure the purity and cleanliness of the electronic gases contained in the steel cylinders, is a technical problem that needs to be solved urgently. Summary of the invention

[0005] The present invention provides a steel cylinder for containing electronic gas and a processing method thereof, which are used to optimize the processing technology of the steel cylinder for containing electronic gas, thereby ensuring the purity and cleanliness of the electronic gas contained in the steel cylinder.

[0006] According to some embodiments, the present invention provides a method for processing a steel cylinder containing electronic gas, comprising the following steps:

[0007] forming a cylinder, the cylinder comprising an inner surface and an outer surface;

[0008] cleaning the inner surface of the cylinder;

[0009] Filling the steel cylinder with electronic gas to be contained, and leaving the steel cylinder to stand for a first preset time;

[0010] The electronic gas to be contained in the steel cylinder is emptied.

[0011] In some embodiments, before cleaning the inner surface of the cylinder, the following steps are also included:

[0012] Performing a first mechanical polishing treatment on the outer surface of the steel cylinder;

[0013] The inner surface of the steel cylinder is subjected to a second mechanical polishing process.

[0014] In some embodiments, the specific steps of cleaning the inner surface of the cylinder include:

[0015] Cleaning the inner surface of the cylinder with a chemical cleaning agent;

[0016] Cleaning the inner surface of the cylinder with pure water;

[0017] Performing electrochemical polishing on the inner surface of the steel cylinder;

[0018] The inner surface of the cylinder is cleaned with pure water.

[0019] In some embodiments, before the electronic gas to be contained is filled into the steel cylinder and the steel cylinder is left to stand for a first preset time, the following steps are also included:

[0020] Perform multiple cycles, the cycles comprising:

[0021] The steel cylinder is subjected to a vacuum treatment;

[0022] Fill the steel cylinder with inert gas.

[0023] In some embodiments, the loop step is performed 50 to 150 times.

[0024] In some embodiments, before the electronic gas to be contained is filled into the steel cylinder and the steel cylinder is left to stand for a first preset time, the following steps are also included:

[0025] The steel cylinder is subjected to a vacuum treatment to exhaust the gas in the steel cylinder.

[0026] In some embodiments, after the electronic gas to be contained in the cylinder is emptied, the following steps are further included:

[0027] Detecting whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements, and if not, refilling the electronic gas to be contained into the steel cylinder, and leaving the steel cylinder to stand for a second preset time, wherein the second preset time is less than or equal to the first preset time;

[0028] The electronic gas to be contained in the steel cylinder is emptied again.

[0029] In some embodiments, after the electronic gas to be contained in the cylinder is emptied again, the following steps are further included:

[0030] Detecting whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements, and if not, refilling the electronic gas to be contained into the steel cylinder, and leaving the steel cylinder to stand for a third preset time, wherein the third preset time is less than or equal to the second preset time;

[0031] The electronic gas to be contained in the steel cylinder is emptied again.

[0032] In some embodiments, after the electronic gas to be contained in the cylinder is emptied, the following steps are further included:

[0033] Check whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements. If so, fill the steel cylinder with inert gas.

[0034] According to other embodiments, the present invention further provides a steel cylinder for containing electronic gas, which is processed by the processing method for the steel cylinder for containing electronic gas as described above.

[0035] The steel cylinder for containing electronic gas and the processing method thereof provided by the present invention, after cleaning the inner surface of the steel cylinder, the electronic gas to be contained is filled into the steel cylinder, and the steel cylinder is left to stand for a first preset time, and then the electronic gas to be contained in the steel cylinder is emptied, thereby passivating the inner surface of the steel cylinder, forming a protective film covering the inner surface of the steel cylinder, thereby isolating the electronic gas subsequently contained in the steel cylinder from the inner surface of the steel cylinder through the protective film, avoiding the contamination of the electronic gas by impurities on the inner surface of the steel cylinder, and avoiding the chemical reaction between the inner surface of the steel cylinder and the electronic gas, thereby ensuring the purity and cleanliness of the electronic gas contained in the steel cylinder. At the same time, since the present invention forms the protective film by standing, there is no need to perform heat treatment or ion implantation on the steel cylinder, which is not only simple to operate and low in cost, but also avoids damage to the steel cylinder caused by heat treatment or ion implantation and the introduction of new impurities to pollute the steel cylinder. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Attached Figure 1 It is a flow chart of a method for processing a steel cylinder containing electronic gas in a specific embodiment of the present invention. DETAILED DESCRIPTION

[0037] The specific implementation methods of the steel cylinder for containing electronic gas and the processing method thereof provided by the present invention are described in detail below with reference to the accompanying drawings.

[0038] This specific embodiment provides a method for processing a steel cylinder containing electronic gas, Figure 1 FIG. 1 is a flow chart of a method for processing a steel cylinder containing electronic gas in a specific embodiment of the present invention. Figure 1 As shown, the method for processing a steel cylinder containing electronic gas comprises the following steps:

[0039] Step S11, forming a steel cylinder, wherein the steel cylinder comprises an inner surface and an outer surface;

[0040] Step S12, cleaning the inner surface of the cylinder;

[0041] Step S13, filling the electronic gas to be contained into the steel cylinder, and leaving the steel cylinder to stand for a first preset time;

[0042] Step S14, emptying the electronic gas to be contained in the steel cylinder.

[0043] In some embodiments, before cleaning the inner surface of the cylinder, the following steps are also included:

[0044] Performing a first mechanical polishing treatment on the outer surface of the steel cylinder;

[0045] The inner surface of the steel cylinder is subjected to a second mechanical polishing process.

[0046] Specifically, after the steel cylinder is manufactured and formed, the outer surface of the steel cylinder is first subjected to the first mechanical polishing treatment to reduce the roughness of the outer surface of the steel cylinder. Then, the inner surface of the steel cylinder is subjected to the second mechanical polishing treatment to reduce the roughness of the inner surface of the steel cylinder.

[0047] In some embodiments, the specific steps of cleaning the inner surface of the cylinder include:

[0048] Cleaning the inner surface of the cylinder with a chemical cleaning agent;

[0049] Cleaning the inner surface of the cylinder with pure water;

[0050] Performing electrochemical polishing on the inner surface of the steel cylinder;

[0051] The inner surface of the cylinder is cleaned with pure water.

[0052] For example, after the second mechanical polishing treatment is performed on the inner surface of the steel cylinder, the chemical cleaning agent is used to clean the inner surface of the steel cylinder to remove impurities on the inner surface of the steel cylinder through chemical reaction. Afterwards, the inner surface of the steel cylinder is cleaned with high-purity pure water to remove impurities on the inner surface of the steel cylinder and unreacted chemical cleaning agent. Next, the inner surface of the steel cylinder is electrochemically polished to further reduce the roughness of the inner surface of the steel cylinder, for example, to reduce the roughness of the inner surface of the steel cylinder to below 0.1 μm. Then, a valve is installed on the steel cylinder, and the valve is used to control the opening and closing of the steel cylinder. Afterwards, the inner surface of the steel cylinder is cleaned again with pure water.

[0053] In some embodiments, before the electronic gas to be contained is filled into the steel cylinder and the steel cylinder is left to stand for a first preset time, the following steps are also included:

[0054] Perform multiple cycles, the cycles comprising:

[0055] The steel cylinder is subjected to a vacuum treatment;

[0056] Fill the steel cylinder with inert gas.

[0057] Specifically, before executing the circulation step, the steel cylinder is first subjected to an airtight pressure test to detect the airtightness of the steel cylinder. After the rigid airtightness meets the requirements, the circulation step is performed multiple times to replace the gas in the steel cylinder to ensure the cleanliness of the steel cylinder. When executing the circulation step, the steel cylinder is first vacuumed to remove the impurity gas in the steel cylinder; and then the inert gas is filled into the steel cylinder. When executing the circulation step for the next time, the steel cylinder is first vacuumed, and the inert gas filled in the previous time will bring out the impurity gas in the steel cylinder during vacuuming, that is, the impurity gas in the steel cylinder will be discharged from the steel cylinder along with the flow of the inert gas. The multiple times mentioned in this specific embodiment refers to more than twice.

[0058] In some embodiments, the cycle step is performed 50 to 150 times, so as to improve the processing efficiency of the cylinder while ensuring the cleanliness of the cylinder. In one example, the cycle step is performed 100 times.

[0059] In some embodiments, before the electronic gas to be contained is filled into the steel cylinder and the steel cylinder is left to stand for a first preset time, the following steps are also included:

[0060] The steel cylinder is subjected to a vacuum treatment to exhaust the gas in the steel cylinder.

[0061] Specifically, the steel cylinder is subjected to a vacuum treatment, and after the gas in the steel cylinder is emptied, the electronic gas to be contained is filled into the steel cylinder, and the steel cylinder is left to stand for a first preset time, so as to passivate the inner surface of the steel cylinder and form a protective film covering the inner surface of the steel cylinder, thereby isolating the electronic gas subsequently contained in the steel cylinder from the inner surface of the steel cylinder through the protective film, thereby preventing the impurities on the inner surface of the steel cylinder from contaminating the electronic gas, and also preventing the inner surface of the steel cylinder from chemically reacting with the electronic gas, thereby ensuring the purity and cleanliness of the electronic gas contained in the steel cylinder. The protective film can be a passivation film generated by the electronic gas to be contained adsorbed on the inner surface of the steel cylinder and chemically reacting with the steel cylinder. After the steel cylinder is left to stand for the first preset time, the gas in the steel cylinder is emptied by vacuuming. In one example, the first preset time is 30 days.

[0062] In some embodiments, after the electronic gas to be contained in the cylinder is emptied, the following steps are further included:

[0063] Detecting whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements, and if not, refilling the electronic gas to be contained into the steel cylinder, and leaving the steel cylinder to stand for a second preset time, wherein the second preset time is less than or equal to the first preset time;

[0064] The electronic gas to be contained in the steel cylinder is emptied again.

[0065] Specifically, after the electronic gas to be contained in the steel cylinder is emptied, it is detected whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements, for example, it is detected whether the indexes such as the purity and cleanliness of the electronic gas to be contained discharged from the steel cylinder meet the preset requirements. If not, it is confirmed that the protective film does not completely cover the inner surface of the steel cylinder or the density of the protective film does not meet the preset density requirements, and the following repeated steps are performed multiple times: the electronic gas to be contained is filled into the steel cylinder; the steel cylinder is emptied. In one example, before the steel cylinder is left to stand for a second preset time, the repeated steps are performed at least 30 times to further ensure the cleanliness of the steel cylinder. After performing the repeated steps multiple times, the electronic gas to be contained is filled into the steel cylinder, and the steel cylinder is left to stand for a second preset time. Setting the second preset time to be less than the first preset time not only improves the processing efficiency of the steel cylinder, but also helps to further improve the cleanliness of the steel cylinder. In one example, the second preset time is 20 days.

[0066] In some embodiments, after the electronic gas to be contained in the cylinder is emptied again, the following steps are further included:

[0067] Detecting whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements, and if not, refilling the electronic gas to be contained into the steel cylinder, and leaving the steel cylinder to stand for a third preset time, wherein the third preset time is less than or equal to the second preset time;

[0068] The electronic gas to be contained in the steel cylinder is emptied again.

[0069] Specifically, after the steel cylinder is left at rest for the second preset time, the steel cylinder is emptied, and the index of the electronic gas to be contained discharged from the steel cylinder is detected again to see if it meets the preset requirements. If not, it is confirmed that the protective film still does not completely cover the inner surface of the steel cylinder or the density of the protective film still does not meet the preset density requirements, and the following repeated steps are performed again for multiple times: the electronic gas to be contained is filled into the steel cylinder; the steel cylinder is emptied. In one example, before the steel cylinder is left at rest for the third preset time, the repeated steps are performed at least 20 times to further ensure the cleanliness of the steel cylinder. After the repeated steps are performed again for multiple times, the electronic gas to be contained is filled into the steel cylinder again, and the steel cylinder is left at rest for the third preset time, so that the protective film more fully covers the inner surface of the steel cylinder or further improves the density of the protective film. Setting the third preset time to be less than the second preset time not only improves the processing efficiency of the steel cylinder, but also helps to further improve the cleanliness of the steel cylinder. In one example, the third preset time is 10 days.

[0070] In some embodiments, multiple repetition steps can be performed within a preset time, and the repetition steps include: step S13, filling the electronic gas to be contained into the steel cylinder, and leaving the steel cylinder to stand for a first preset time; step S14, emptying the electronic gas to be contained in the steel cylinder. After each execution of the repetition step, it is detected whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements. If not, the next repetition step is performed until the preset time is reached or the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements. In one example, for two repetition steps performed successively, the time for leaving the steel cylinder to stand in the first repetition step is greater than or equal to the time for leaving the steel cylinder to stand in the later repetition step. By performing the repetition step multiple times, the cleanliness of the steel cylinder can be better ensured, thereby ensuring the purity and cleanliness of the electronic gas contained in the steel cylinder.

[0071] In some embodiments, after the electronic gas to be contained in the cylinder is emptied, the following steps are further included:

[0072] Check whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements. If so, fill the steel cylinder with inert gas.

[0073] Specifically, after confirming whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements, 0.2MPa of inert gas is filled into the steel cylinder, thereby maintaining the cleanliness of the steel cylinder and ensuring the safety of the steel cylinder.

[0074] This specific embodiment also provides a steel cylinder for containing electronic gas, which is processed using the processing method for the steel cylinder for containing electronic gas as described above.

[0075] The steel cylinder for containing electronic gas and the processing method thereof provided in this specific embodiment, after cleaning the inner surface of the steel cylinder, the electronic gas to be contained is filled into the steel cylinder, and the steel cylinder is left to stand for a first preset time, and then the electronic gas to be contained in the steel cylinder is emptied, thereby passivating the inner surface of the steel cylinder and forming a protective film covering the inner surface of the steel cylinder, thereby isolating the electronic gas subsequently contained in the steel cylinder from the inner surface of the steel cylinder through the protective film, avoiding contamination of the electronic gas by impurities on the inner surface of the steel cylinder, and avoiding chemical reaction between the inner surface of the steel cylinder and the electronic gas, thereby ensuring the purity and cleanliness of the electronic gas contained in the steel cylinder. At the same time, since the protective film is formed by standing in this specific embodiment, there is no need to perform heat treatment or ion implantation on the steel cylinder, which is not only simple to operate and low in cost, but also avoids damage to the steel cylinder caused by heat treatment or ion implantation and pollution of the steel cylinder caused by the introduction of new impurities.

[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for treating a steel cylinder containing electronic gas, characterized in that: The steps include: forming a cylinder, the cylinder comprising an inner surface and an outer surface; cleaning the inner surface of the cylinder; Filling the steel cylinder with electronic gas to be contained, and leaving the steel cylinder to stand for a first preset time; The electronic gas to be contained in the steel cylinder is emptied.

2. The method for processing a steel cylinder for containing electronic gas according to claim 1, characterized in that: Before cleaning the inner surface of the cylinder, the following steps are also included: Performing a first mechanical polishing treatment on the outer surface of the steel cylinder; The inner surface of the steel cylinder is subjected to a second mechanical polishing process.

3. The method for processing a steel cylinder for containing electronic gas according to claim 1, characterized in that: The specific steps of cleaning the inner surface of the cylinder include: Cleaning the inner surface of the cylinder with a chemical cleaning agent; Cleaning the inner surface of the cylinder with pure water; Performing electrochemical polishing on the inner surface of the steel cylinder; The inner surface of the cylinder is cleaned with pure water.

4. The method for processing a steel cylinder for containing electronic gas according to claim 1, characterized in that: Before the electronic gas to be contained is filled into the steel cylinder and the steel cylinder is left to stand for a first preset time, the following steps are also included: Perform multiple cycles, the cycles comprising: The steel cylinder is subjected to a vacuum treatment; The cylinder is filled with inert gas.

5. The method for processing a steel cylinder for containing electronic gas according to claim 4, characterized in that: The number of times the cycle step is executed is 50 to 150 times.

6. The method for processing a steel cylinder for containing electronic gas according to claim 1, characterized in that: Before the electronic gas to be contained is filled into the steel cylinder and the steel cylinder is left to stand for a first preset time, the following steps are also included: The steel cylinder is subjected to a vacuum treatment to exhaust the gas in the steel cylinder.

7. The method for processing a steel cylinder for containing electronic gas according to claim 1, characterized in that: After the electronic gas to be contained in the steel cylinder is emptied, the following steps are also included: Detecting whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements, and if not, refilling the electronic gas to be contained into the steel cylinder, and leaving the steel cylinder to stand for a second preset time, wherein the second preset time is less than or equal to the first preset time; The electronic gas to be contained in the steel cylinder is emptied again.

8. The method for processing a steel cylinder for containing electronic gas according to claim 7, characterized in that: After the electronic gas to be contained in the steel cylinder is emptied again, the following steps are also included: Detecting whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements, and if not, refilling the electronic gas to be contained into the steel cylinder, and leaving the steel cylinder to stand for a third preset time, wherein the third preset time is less than or equal to the second preset time; The electronic gas to be contained in the steel cylinder is emptied again.

9. The method for processing a steel cylinder for containing electronic gas according to claim 1, characterized in that: After the electronic gas to be contained in the steel cylinder is emptied, the following steps are also included: It is detected whether the index of the electronic gas to be contained discharged from the steel cylinder meets the preset requirements. If so, an inert gas is filled into the steel cylinder.

10. A steel cylinder for containing electronic gas, characterized in that: The method for treating a steel cylinder for containing electronic gas as claimed in claim 1 is adopted.

Citation Information

Patent Citations

  • Method for cleaning steel cylinder of trichlorosilane in electronic pouring in level

    CN101050541A

  • Gas cylinder treatment system for ultra-pure gas and treatment method thereof

    CN111469042A

  • Processing method of electronic-grade chlorine trifluoride packaging steel cylinder

    CN113005389A

  • Heat treatment passivation method for steel cylinder special for special gas

    CN115029657A

  • Passivating treatment method for steel bottle for storing electronic-grade boron trichloride

    CN115074656A