Three-dimensional solar evaporation material and preparation method, application and testing device and method thereof

Silicon carbide ceramic materials are prepared through femtosecond laser processing, and multiple parallel grooves and micro-nano structures are used to enhance light absorption and wetting performance to form an efficient white water film, solving the problems of low evaporation rate and corrosiveness of existing solar evaporation materials. Efficient seawater desalination and renewable energy applications have been achieved.

CN119043984AInactive Publication Date: 2024-11-29CHONGQING UNIV OF POSTS & TELECOMM

Patent Information

Application Number
CN202411151964.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The evaporation rate of existing solar evaporation materials is limited by the thermodynamic limit. Three-dimensional structural interface evaporators have not yet fully utilized the multiple refraction and capture of light, and common materials are prone to corrosion in seawater, affecting service life and efficiency.

Method used

Silicon carbide ceramic materials with multiple parallel grooves and micro-nano structures are prepared by femtosecond laser processing. By adjusting the micro-nano structure size, the light absorption and wetting performance is enhanced, and an efficient white water film is formed to increase the evaporation rate and absorb water through water. Line-regulate the water film thickness to improve evaporation efficiency.

Benefits of technology

Silicon carbide materials that achieve high evaporation performance and strong wetting performance under dark conditions have increased 270 times the evaporation rate. The material has good corrosion resistance and high thermal conductivity, and is suitable for seawater desalination and renewable energy fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119043984A_ABST
    Figure CN119043984A_ABST
Patent Text Reader

Abstract

The invention discloses a three-dimensional solar evaporation material and a preparation method, application and testing device and method thereof, and the preparation method comprises the following steps: 1) polishing and cleaning a silicon carbide ceramic wafer, and fixing the silicon carbide ceramic wafer on a displacement platform for femtosecond laser processing; 2) processing the surface of the silicon carbide ceramic wafer by using a femtosecond laser, controlling the material to move through a displacement platform, and processing under a processing area to obtain a water absorption line; and (3) a series of grooves which are arranged in parallel and have the depth of 20 microns and the distance between every two adjacent grooves of 120 microns are obtained, the grooves are rich in micro-nano structures, the sizes of the micro-nano structures span five orders of magnitude, and each micro-nano structure is further provided with a water absorption line with the width of 200 microns and the depth of 60 microns. When the prepared material is vertically placed, a stable white high-evaporation-rate water film accounting for 25% of the total water film area is provided. Under the illumination of 1-4 sunlight, a white film with a high evaporation rate always exists, good wettability and evaporation performance are kept, meanwhile, the corrosion resistance and the high sunlight absorptivity are achieved, and the film can be applied to the fields of seawater desalination, steam power generation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar evaporation materials, and in particular to a testing device and method for a silicon carbide ceramic material having super wettability and strong evaporation performance at 100°C. Background Art

[0002] The increasing shortage of fresh water caused by global climate change, socio-economic development, rapid population growth, urbanization and water pollution is one of the most serious global challenges facing the world today. To solve the problem of water shortage, scientific and technological breakthroughs are needed in the fields of desalination, wastewater reuse and improving water resource utilization efficiency. Fresh water production technology involves a large amount of energy. At present, the desalination industry consumes about 75 terawatt-hours of electricity per year, accounting for about 0.4% of the world's electricity generation. However, fossil fuel steam power plants and nuclear power plants require 75,000-450,000 liters of water for each megawatt-hour of electricity generation. This relationship between water and energy, known as the water-energy relationship, has made the development of water treatment technology based on renewable energy the mainstream choice in the world today. At present, evaporators used in solar water evaporation processes generally adopt one-dimensional interfacial evaporation structures, which mainly use porous, interfacial structure-free materials floating on the water surface to distill seawater. However, the maximum evaporation rate of this structure is limited by the thermodynamic limit of solar energy utilization. In contrast, three-dimensional structured interfacial evaporators have higher potential because they can use surface structures for multiple refraction and capture of light and interact with environmental energy. This property enables the 3D structured interface evaporator to achieve higher solar evaporation rates and energy utilization efficiency. Studies have shown that the 3D structured interface evaporator can provide a 130-fold increase in evaporation rate compared to natural evaporation through surface nano / microstructures. Using a similar approach, we studied the effect of water film thickness on the layered surface 6H-SiC nano / microstructure on the water evaporation rate and discovered the effect of white strong evaporation, which increased the evaporation rate by 330 times. Compared to common optical effects, most rough surfaces are darker when wet, however, the wet surface of this material is whiter than the dry surface, similar to the light scattering of clouds in the sky. Based on our discovery of the white strong evaporation phenomenon, we designed a 3D interface dark / solar evaporator material for water purification / seawater desalination technology.

[0003] When the sponge-like material floats on the water surface to evaporate, its internal pores are prone to accumulation of impurities, which affects the continuous water supply and reduces the evaporation efficiency. At the same time, metal evaporators are exposed to corrosive substances such as seawater for a long time, and need to be replaced regularly, with high maintenance costs. Therefore, high thermal conductivity ceramic materials with excellent thermal conductivity and good corrosion resistance have potential for application in solar evaporators. The high thermal conductivity of ceramic materials can effectively transfer heat to the evaporation surface, provide more heat, and promote the rapid evaporation of water. In addition, high thermal conductivity ceramic materials also have good corrosion resistance and can operate stably for a long time under harsh environmental conditions. In contrast, metal materials are easily affected by corrosion and oxidation, which limits the service life and performance stability of the evaporator. The micro-nano structure with regular micro-grooves on the surface manufactured by femtosecond laser micro-nano manufacturing technology can make silicon carbide materials have super hydrophilicity and wicking properties. At the same time, the micro-nano structure on the surface can greatly increase the actual surface area and the capture rate of external energy, thereby increasing the evaporation rate of water. In the case that the absorption rate of sunlight by existing materials has reached a bottleneck, the water evaporation rate can still be significantly increased by improving the wettability of the material.

[0004] The evaporation rate of existing solar evaporation materials is calculated based on the mass loss per second divided by the wetted area. The wetted area here generally refers to the projected area. In order not to calculate the wetted area, some studies decompose the mass loss per second into the wetted area multiplied by the water film height multiplied by the density, and then deduct the wetted area and only calculate the change trend of the water film height over time. However, this secondary calculation method has a large error. In contrast, most experiments use electronic balances to obtain the lost mass, and use image processing technology (such as digital camera shooting and software analysis) or contact / non-contact measuring instruments (such as laser scanners) to measure the wetted area.

[0005] In view of this, this application is hereby filed. Summary of the invention

[0006] The present invention realizes a silicon carbide material with high evaporation performance and strong wetting performance under dark conditions. At the same time, due to its unique three-dimensional surface micro-nano structure that can enhance light absorption, its evaporation performance under solar conditions is also excellent, and the strong wicking properties provided by the micron-level surface V-shaped grooves remain stable under light conditions. Through evaporation experiments at room temperature, the present invention finds that there is a white water film area with high evaporation performance when water evaporates on the material. The white water film is due to the strong light scattering of small water droplets distributed on the surface of the structure. The appearance of small water droplets prolongs the three-phase contact line and enhances the evaporation performance of the material. The ratio of the white water film to the wetted area of ​​the material of the present invention is stable at 25% under vertical placement and different solar light intensities, and the evaporation performance is excellent. The absorption effect of the photothermal material at different wavelengths is directly related to the size of the micro-nano structure, so the size of the micro-nano structure can be adjusted to enhance light absorption. In addition, the rich micro-nano structure greatly increases the heat exchange area between the photothermal material and water. The increase in bubble activation nucleation in the micro-nano gap will also lead to an increase in bubbles for heat exchange, but the microstructure can reduce the separation resistance of the bubbles. The above factors greatly promote the formation and separation of bubbles, thereby improving the heat transfer coefficient of the material. The micro-nanostructure can also improve the wetting properties of the material, and its micro-gaps can also serve as numerous vapor transmission channels. Its porous structure scatters and absorbs sunlight, giving the material considerable light absorption, heat conversion, water and vapor transmission potential.

[0007] Silicon Carbide (SiC) is a semiconductor material with excellent physical and chemical properties. Compared with traditional silicon materials, silicon carbide has higher breakdown voltage, higher electron migration speed and lower conduction loss. This makes silicon carbide advantageous in special working environments such as high temperature, high pressure and high frequency. Silicon carbide also has high thermal conductivity and chemical stability, which makes it widely used in high-power electronic devices, power converters, high-temperature electronic devices and radio frequency electronic devices. In addition, silicon carbide also has good mechanical strength and corrosion resistance. These properties enable it to be used in solar desalination and can ensure the stable operation of the desalination process.

[0008] Superhydrophilic silicon carbide has high interfacial thermal conductivity and can be used as a photothermal material to achieve high evaporation. Experimental and numerical studies have elucidated the main parameters of nanoscale interfacial heat transport, which are (1) interfacial bonding (2) mismatch of vibrational energy carriers (3) surface roughness and (4) interfacial liquid structure. The formation of high-density bands observed on the surface of silicon carbide confirms the ice-like behavior of small water clusters. The formation of ice-like structures explains the large thermal conductivity of silicon carbide. In addition, the solid-water interface thermal conductivity of silicon carbide material is linearly related to the adhesion work (Wa), where Wa~1+cos(a), a is the contact angle. There are two different water distributions in rocks. One is that water only covers the surface of the rock and cannot fill the gap between the two rocks. The other is that water completely fills the gap between the two rocks. In rocks, when the rock has a higher surface energy, the hydrated ions in the water are distributed on the surface of the rock, so the electric potential of the water is very high at this time. The farther away from the rock, the lower the theoretical potential of water and it is electrically neutral. When the surface energy of the rock is low, the hydrated ions in the water will still be distributed on the surface of the rock, but the total amount of hydrated ions adsorbed will be greatly reduced. At this time, the points far away from the substrate surface quickly reach neutrality. When it is reduced to a critical value, due to the electrical layer effect between the water film and the air, the critical layer between the water film and the air will still absorb a certain number of hydrated ions. The theoretical potential of water will also increase as the distance between air and water decreases. Therefore, for rocks with low surface energy, the potential of the water film decreases and then increases, so that a micro-nano water film can be formed on the rock. In view of this, a three-dimensional solar silicon carbide ceramic material with a high evaporation rate at room temperature / solar energy was processed, with an extremely thin water film and a white water film accounting for 25%. It was obtained by femtosecond laser processing. The optimal structure was obtained by changing the laser energy density, scanning speed, processing step length and other parameters, and the optimal evaporation water film (white high evaporation water film accounting for 25%) was obtained by controlling the water inlet. The white water film comes from the strong light scattering, which proves that the density distribution in the micro-nano structure is uneven, and a situation similar to the evaporation of water on rocks occurs (the water does not completely fill the pores formed by the rock), which confirms that when water is distributed on the cactus-like micro-nano structure, an extremely thin micro-nano water film layer will be formed. Due to the low thermal resistance of the thin water film layer, the evaporation rate will be improved. The overall micro-grooves have a high surface energy, which will quickly spread the droplets covering it to form a water film layer, increase the evaporation surface area, and thus increase the evaporation rate. The surface energy of solids can be changed by micron or nano-sized structures. When this surface energy changes, the wetting behavior of the liquid changes, and therefore, the fluid flow process on the surface changes. Micron- and nano-scale structures can also increase the thickness of the adsorption film and increase the hydrodynamic slip at the solid-liquid interface. Microscale structures enhance the capillary driving force. The viscous resistance of water in nanoscale structures is high, but the transport channel is short, which can reduce the thickness of the water film. The advantage of the layered surface structure is that the maximum evaporation performance can be obtained.

[0009] In view of this, the technical solution adopted by the present invention is: a three-dimensional solar evaporation material, having a plurality of parallel and continuously distributed grooves on its surface, the depth of the grooves being 20 μm, the spacing between adjacent grooves being 120 μm, and the grooves being rich in micro-nano structures, the sizes of which span 5 orders of magnitude, and also including a water absorption line.

[0010] Furthermore, the water absorption line is arranged directly below the processing area, and different evaporated water films can be obtained by controlling the depth of the water absorption line entering the water container. The width of the water absorption line is 200 μm and the depth is 60 μm.

[0011] A method for preparing a three-dimensional solar evaporation material comprises the following steps:

[0012] (1) grinding and cleaning the silicon carbide ceramic sheet, and fixing the silicon carbide ceramic sheet on a displacement platform for femtosecond laser processing;

[0013] (2) A femtosecond laser is used to process the surface of a silicon carbide ceramic sheet. The material movement is controlled by a displacement platform. The same laser energy and scanning speed are used to process the surface directly below the processing area twice to obtain a water absorption line.

[0014] Specifically, the processing parameters of the femtosecond laser are: laser energy density 10.6 J / cm 2 , the step length between scanning lines is 120μm, and the scanning speed is 0.2mm / s.

[0015] Specifically, the processing environment of the femtosecond laser is a temperature of 24° C. and a relative humidity of 50%.

[0016] Furthermore, the original silicon carbide ceramic material was purchased from Guangzhou Beilong Electronics Co., Ltd. and the density was as high as 3.12 g / cm 3 , purity is 98.5%, thermal conductivity is 148w m -1 k -1 The highest high temperature resistance can reach 1600℃, the Rockwell hardness is greater than 93HRA, and the elastic modulus is 415GPa.

[0017] The silicon carbide ceramic material with strong evaporation performance under room temperature / solar energy of the present invention has a series of parallel arranged grooves with a depth of 20 μm and a groove spacing of 120 μm, and the grooves are rich in micro-nano structures (micro-nano holes, micro-nano periodic structures, micro-nano flowers), and the sizes of these micro-nano structures span 5 orders of magnitude, so that the surface of the processed silicon carbide ceramic material presents a dark blue color. The special structure makes the water film covering it present two forms, with a white water film that can bring high evaporation. A water absorption groove with a width of 200 μm and a depth of 60 μm is processed directly below the processing area, and different evaporation water films can be obtained by controlling the depth of the water absorption line entering the water container. This control method increases the area of ​​the white water film and brings high evaporation performance. This unique structure brings high light absorption rate, high wettability, and strong evaporation performance. The high wettability enables the material to continuously generate a water film for evaporation under different light, and has stability. The high light absorption rate and strong evaporation performance make the material have great potential in the fields of renewable energy reuse and seawater desalination.

[0018] In addition, the silicon carbide ceramic material of the present invention has strong evaporation performance at room temperature / solar energy, strong corrosion resistance and high thermal conductivity. Under different light conditions, it can quickly respond to thermal energy and ensure uniform temperature distribution on the photothermal surface. Its excellent wetting ability can stably provide efficient evaporation.

[0019] When the surface of the material prepared by the present invention is covered with water film, the water film can be divided into black water film and white water film. This processing parameter can provide a stable white water film with high evaporation rate accounting for 25% of the total water film area when the material is placed vertically.

[0020] The application of the three-dimensional solar evaporation material prepared by the present invention includes the photothermal material that can be used to prepare seawater desalination. The photothermal material can improve the solar evaporation rate and energy utilization efficiency by means of multiple refractions of light and the capture and utilization of environmental energy. The three-dimensional photothermal evaporation system using micro-nano pores has enhanced light absorption, heat conversion, water and steam transmission capabilities, can efficiently generate steam, and is applied to seawater desalination, steam work, etc.

[0021] The three-dimensional solar evaporation material under room temperature / solar energy of the present invention can still maintain good wettability under the illumination of four suns and has a white film that brings a high evaporation rate. Therefore, when applied in the field of seawater desalination, the long-term stable operation of the photothermal material can be guaranteed.

[0022] The present invention also provides another application of photothermal materials, which is applied in the field of renewable energy, and specifically applied in converting solar steam into mechanical energy.

[0023] The room temperature / solar energy three-dimensional solar evaporation material of the present invention has good corrosion resistance and is not easily oxidized, and has a high solar light absorption rate and evaporation rate on the surface. Therefore, it can be applied to the fields of utilizing solar energy to evaporate seawater to produce distilled water, photovoltaic power generation, etc.

[0024] The present invention provides a three-dimensional solar evaporation material evaporation rate test device at room temperature, comprising a high-precision balance, a windshield built around the high-precision balance, a high-speed camera looking down is placed on the top of the windshield, a high-speed camera looking sideways is placed on the outside of the windshield, a needle for controlling the volume of liquid is hung above the tray of the balance, a sample material is placed on the tray of the balance, the center point of the sample material is placed under the needle, and the distance between the sample material and the needle is adjusted so that the droplet hanging on the needle just touches the sample material; the balance is connected to a computer to print the mass of the material and water in real time, and the high-speed camera looking down and the high-speed camera looking sideways are connected to the computer. An LED lamp can be arranged on the inside of the windshield as a supplementary light source, or it can be arranged on the outside of the windshield.

[0025] The top-view camera photographs the wetted area at a speed of 50 frames per second. The photographed pictures are processed with XARA software to obtain the ratio of the wetted area to the processed area, and the ratio is multiplied by the actual processed area to obtain the actual wetted area.

[0026] The windshield is used to reduce the influence of air flow on the balance reading, the high-speed camera is used to monitor the change of the wet area during evaporation, and the use of the LED light source is more conducive to the high-speed camera to observe the light reflection of different air-water interfaces.

[0027] The use of the above high-precision balance can accurately obtain the mass of evaporation at each moment. The addition of the top-view camera provides an opportunity to measure the accurate wet area. The side-view camera captures the shape of the water film at different moments, making it easier to understand the evaporation process on the micro-nano structure. Lighting from different directions provides evidence that the white water film comes from the scattering of light. By using the above evaporation rate measurement device, it is possible to visualize which evaporation rate corresponds to different water film states, making the meniscus evaporation theory more specific and providing insights into obtaining a water film with a high evaporation rate.

[0028] The present invention also provides a method for measuring the evaporation rate of a three-dimensional solar evaporation material at room temperature using the above device, comprising the following steps:

[0029] 1) Set the volume of deionized water, turn on the balance printing function, and start recording with a high-speed camera at 50 frames per second;

[0030] 2) Drop a 15 μl droplet into the material, which quickly spreads as a water film on the surface of the material. Wait for the droplet to evaporate completely and stop recording and printing.

[0031] 3) Measure the mass m1 of the droplet that decreases per second, and obtain the projected wetted area s1 at the corresponding time point through image processing;

[0032] 4) The side-view high-speed camera focuses on the material surface when the water drop just drips in, because the water film is the thickest at the location where the water drop drips in. The camera can capture the interface state during the evaporation time, and the captured image is used to visualize the effect of water film thickness on evaporation rate;

[0033] 5) Calculate the evaporation rate of the silicon carbide ceramic material sample at each time point when it is placed horizontally according to the formula: v = m1 .

[0034] s1

[0035] Five groups of horizontal droplet evaporation experiments were conducted under the experimental conditions of room temperature 24℃ and humidity 50±2% to evaluate the effect of water film thickness on evaporation rate. The main device of the experiment is a high-precision balance with a measurement accuracy of 0.00001. The processed hydrophilic silicon carbide material is placed on this balance. A 15μl deionized water droplet is sent to the central area of ​​the material through a syringe pump, and a high-speed camera is used to monitor the diffusion of water droplets on the material in real time. The computer connected to the balance prints out the current balance reading every second. Droplets are added to the surface of the material, and then the wetting area and mass loss of the droplets on the surface of the material at each moment are calculated. This method is universal when the material temperature is less than 100℃. The thickness of the water film will gradually become thinner as the evaporation process proceeds, and the thickness of the water film affects the evaporation rate. The evaporation of the meniscus can be divided into three regions: adsorption layer, thin film evaporation stage, and intrinsic meniscus stage. The evaporation of the adsorption layer occurs at the nanoscale, the evaporation of the thin film area occurs at the micrometer scale, and the evaporation on the intrinsic meniscus occurs at the macroscale. Affected by the microscopic thickness of the liquid film, the evaporation rate in the evaporation area of ​​the thin film is the highest, while the adsorption layer cannot evaporate due to the attraction between the solid and the liquid and the vapor pressure. In thin film evaporation, surface roughness affects both separation pressure and flow permeability, and surface roughness also affects the thickness distribution and heat transfer effect of the evaporating film. The silicon carbide ceramic material of the present invention increases the evaporation rate by 270 times. This super-strong evaporation point occurs at the moment when the all-white water film evaporates, near the end of the evaporation process. Compared with common optical effects, most rough surfaces are darker when wet, but the wet surface of this material is whiter than the dry surface, similar to the light scattering of clouds in the sky. In order to utilize the strong evaporation characteristics of the white water film, the present invention finds the structure with the best white film ratio by modifying the processing parameters.

[0036] The present invention also provides a three-dimensional solar evaporation material evaporation rate testing device under solar energy, comprising a high-precision balance, a water container, a high-speed camera, a xenon lamp, a filter, a lens and an aperture. The light emitted by the xenon lamp is irradiated onto the surface of the material through the filter, the lens and the aperture; the material is fixed by a fixing device and placed vertically in the water container, the water container and the material are placed on a high-precision balance, the mass of water evaporated in each time period is recorded, the balance is connected to a computer, and the mass of the material and the water is printed in real time.

[0037] When the experiment was conducted using the above device, the room temperature was 24°C, the relative humidity was 50%, and there was no wind.

[0038] The above device can be used to obtain stable power sunlight irradiation and a thinner steady-state water film, while eliminating the error caused by light heating the water matrix and air.

[0039] Finally, the present invention provides a method for measuring the evaporation rate of three-dimensional solar evaporation materials under solar energy using the above device, comprising the following steps:

[0040] 1) Place the material vertically in a water container. The capillary force of the material is greater than the gravity. At this time, the water in the water container will be pumped to the surface of the material. When the gravity of the pumped water is balanced with the capillary force, the height of the water film hardly changes. Turn on the xenon light source and wait until the light intensity and the vertically spread water film are stable. Then record the current balance reading m2;

[0041] 2) Wait for time t and record the balance reading m3;

[0042] 3) Calculate the mass loss of water in the water container within the time period, obtain the projected wet area s1 of the corresponding time period through image processing, process the captured image with XARA software, obtain the ratio of the wet area to the processing area, multiply the ratio by the actual processing area to obtain the actual wet area s1;

[0043] 4) Calculate the average evaporation rate of silicon carbide ceramic material samples under different light intensities when placed vertically according to the formula:

[0044] The strong evaporation silicon carbide ceramic material of the present invention has a light absorption rate of up to 98%. Therefore, in order to test and verify the bright prospects of the strong evaporation silicon carbide ceramic material of the present invention in the field of seawater desalination, the present invention provides a test method for the evaporation rate of the above-mentioned strong evaporation silicon carbide ceramic material under different solar light intensities. First, the material is placed vertically in a water container. Due to the interference of gravity, the thickness of the water film in this placement method is thinner than that of the water film placed horizontally. The water container is placed on a balance together with the material. When the capillary force is balanced with the gravity, the water film no longer expands, and an evaporation water film of stable thickness is obtained at this time. At the same time, the reading of the balance is monitored at this moment. Compared with the reading at the end of the observation, the amount of evaporated water can be calculated, thereby obtaining the evaporation rate. The light emitted by the xenon lamp is irradiated on the surface of the material through a filter, a lens and an aperture. Changing the input current can accurately simulate the irradiation of sunlight of different intensities. The AM1.5G filter is used to simulate the solar spectrum, and the aperture and lens are used to control the sunlight to irradiate in the processing area. The thickness of the water film, the flow behavior of the water film and the white film are recorded and observed with a high-speed camera. This device is convenient for measuring the evaporation rate under different light intensities. Through measurement, it is found that the proportion of white water film in the highly evaporative silicon carbide ceramic material of the present invention can reach up to 25%. Compared with when the proportion of white water film is about 10% under 0 sunlight, the evaporation rate is increased by 3 times.

[0045] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0046] 1. A method for producing a silicon carbide ceramic material with strong evaporation performance at room temperature / solar energy provided by an embodiment of the present invention. The surface of the super-wetting and strong evaporation silicon carbide ceramic material is processed into grooves with a micron structure by femtosecond laser, which has a capillary pumping effect and excellent wetting performance, and stably supplies water to the evaporation surface to provide continuous high evaporation; the abundant micro-nano pores, nanospheres, and periodic micro-nano structures are conducive to increasing the evaporation area, reducing thermal resistance, and achieving the purpose of efficient evaporation;

[0047] 2. The embodiment of the present invention provides a silicon carbide ceramic material with strong evaporation performance at room temperature / solar energy, and has a white water film with a stable high evaporation rate. This water film always exists in the vertical stable water film state, and when the light intensity is increased, the ratio of the white water film to the wetted area remains unchanged, which improves the stable high evaporation of the material and has prospects in the field of water desalination.

[0048] 3. A silicon carbide ceramic material with super wettability provided in an embodiment of the present invention has good corrosion resistance and is not easily oxidized, and has a high solar light absorption rate on the surface, so it can be applied to the fields of using solar energy to evaporate seawater to produce distilled water, photovoltaic power generation, etc.;

[0049] 4. The testing device and method for silicon carbide ceramic materials with strong evaporation performance at room temperature provided by the embodiment of the present invention optically visualizes the micro-nanostructure diagram of the water-air interface corresponding to the evaporation rate points at different evaporation moments, and verifies that the phenomenon of white water film comes from light scattering by lighting from all directions of LED. The testing device and method for silicon carbide ceramic materials with strong evaporation performance under different solar light intensities provided by the embodiment of the present invention utilizes capillary force to transport the working liquid to the evaporation surface, controls the mass loss read by the balance to only come from the evaporation of the liquid on the evaporation surface, and adjusts the current to control the light intensity vertically incident on the evaporation surface, so that the evaporation rate of the stable water film can be measured quickly and conveniently.

[0050] 5. Compared with other evaporation rate test devices that use a balance with an accuracy of 0.0001g, our evaporation rate test device uses a high-precision balance with an accuracy of 0.00001g, and uses image processing technology to intuitively and accurately obtain the evaporation rate. When the material is placed vertically to measure the evaporation rate, compared with other experiments that directly stick the material in the foam and then place it in a water container, our experiment suspends the material to eliminate the damage to the material structure caused by the friction between the foam and the material. At the same time, the suspension method makes it easy to adjust the height of the material immersed in the water, making it easy to control the amount of water inlet. Finally, the suspension material also prevents the interaction between the material and the fixed object from affecting the balance reading.

[0051] 6. Meniscus evaporation is divided into three regions, each with a different thermal resistance. The overall thermal resistance of the adsorption film is actually infinite because there is no evaporation in this region. Due to the relatively thick liquid film, the resistance of the inherent meniscus region can also be very high. The thermal resistance reaches a minimum in the transition zone. In this region, the relatively thin liquid film thickness imposes a moderate thermal resistance. In terms of material preparation, the microscale structure enhances the capillary driving force, the viscous resistance of water in the nanoscale structure is high, but the transport channel is short, which can reduce the thickness of the water film. The advantage of the layered surface structure is that the maximum performance can be obtained during the phase change process. Therefore, the present invention proposes to control the thickness of the water film in the transition region to obtain a water film with a high evaporation rate. In order to obtain the above-mentioned water film, we proposed two solutions, one is to control the water inflow and thus control the thickness of the water film, and the other is a new material processing method. In this processing method, we use femtosecond laser to bombard the target material, leaving a groove with a depth of about 20μm on the surface of the material for capillary driven water supply. Due to Coulomb explosion, numerous micro-nano protrusions similar to the cactus structure are formed on the wall of the groove, and the top of the protrusion contains white silica nanospheres ( Figure 1). In this super-hydrophilic hierarchical structure, the micro-nano channels on the wall have strong flow resistance, and the water flowing in the microgrooves will be pumped by the wall structure and form a thin water film on the groove wall. When adjusting the processing parameters, we found that with a laser energy density of 10.6J / cm2, a step length of 120μm between scanning lines, and a scanning speed of 0.2mm / s, the processed material has a rich nanostructure, and the evaporation rate test results also show the excellent evaporation performance of this material. At the same time, we found the white water film with the largest area that brings a high evaporation rate under this processing parameter ( Figure 4 b), it also exists when the surface temperature of the material rises and its area remains unchanged. By consulting the literature and observing with a high-power optical microscope, it is found that ( Figure 3 (b1)-(b9)), this white water film is due to the light scattering caused by the uneven density of water in the pores, which shows that the continuous water film of water in the micro-nano pores is split and exists in the form of small water droplets. The numerous independent small water films lead to the extension of the three-phase contact line, which promotes high evaporation. Compared with the material in patent CN116174926A, the material of the present invention has a richer nanostructure and better evaporation performance, and has a large-area high-evaporation white water film that it does not have. The addition of water absorption lines enables the material of the present invention to have the ability to regulate the thickness of the water film, further optimizing the material in CN116174926A. We compared the evaporation rates of the material of the present invention and the material in patent CN116174926A at different temperatures when the materials are placed vertically, and the results are as follows Figure 4 c. Under the condition of no wind speed, the material of the present invention with a white film ratio of 25% obtained 34 μg cm at 20°C, 40°C, 60°C, and 80°C respectively. -2 s -1 , 96 μg cm -2 s -1 , 200 μg cm -2 s -1 , 235 μg cm -2 s -1 In contrast, the material prepared by patent CN116174926A only obtained 18.16 μg cm at the above four temperatures and a wind speed of 0.5 m / s. -2 s -1 , 22 μg cm -2 s -1 , 34 μg cm -2 s -1 , 44 μg cm -2 s -1 The evaporation rate of the material of the present invention has excellent evaporation performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0053] Figure 1 The surface 3D image and SEM (scanning electron microscope) image of the strongly evaporated silicon carbide ceramic material provided by the embodiment of the present invention;

[0054] Figure 2 The absorptivity of silicon carbide ceramic materials at different wavelengths provided by the embodiments of the present invention;

[0055] Figure 3 The embodiment of the present invention provides a process of diffusion and evaporation of a droplet on the surface of a strong evaporating silicon carbide ceramic material at room temperature, specifically providing a relationship between the evaporation rate and time, and a relationship between the evaporation rate and the shape of the air-water interface.

[0056] Figure 4 The evaporation rate of the liquid on the surface of the superwet silicon carbide ceramic material provided by the embodiment of the present invention. Figures a, b, c, and d are respectively the optical graph of 10% white film area, the optical graph of 25% white film area, the evaporation rate comparison graph with patent CN116174926A, and the evaporation rate comparison graph of the liquid on the surface of the superwet silicon carbide ceramic material with different white film areas under different solar intensities;

[0057] Figure 5 Figure 1 (a) shows a normal temperature test device for testing evaporation rate and a schematic diagram of the solar device structure (b) provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0058] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0059] In the following description, a large number of specific details are set forth in order to provide a thorough understanding of the present invention. However, it is apparent to those of ordinary skill in the art that these specific details do not have to be employed to practice the present invention. In other embodiments, in order to avoid confusing the present invention, well-known structures are not specifically described.

[0060] Throughout the specification, references to "one embodiment," "an embodiment," "an example," or "an example" mean that a particular feature, structure, or characteristic described in conjunction with the embodiment or example is included in at least one embodiment of the present invention. Therefore, the phrases "one embodiment," "an embodiment," "an example," or "an example" appearing in various places throughout the specification do not necessarily all refer to the same embodiment or example. In addition, particular features, structures, or characteristics may be combined in one or more embodiments or examples in any suitable combination and / or sub-combination. In addition, it will be appreciated by those of ordinary skill in the art that the figures provided herein are for illustrative purposes and that the figures are not necessarily drawn to scale. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0061] In the description of the present invention, the directions or positional relationships indicated by terms such as “front”, “rear”, “left”, “right”, “up”, “down”, “vertical”, “horizontal”, “high”, “low”, “inside” and “outside” are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention and simplifying the description. They do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they should not be understood as limiting the scope of protection of the present invention.

[0062] Example 1

[0063] The embodiment of the present invention provides a silicon carbide ceramic material with strong evaporation performance. The silicon carbide ceramic material is characterized by a 3D confocal microscope to have a series of parallel grooves with a depth of 20 μm and a spacing of 120 μm between adjacent grooves, and its SEM image shows that the grooves are rich in micro-nano structures (micro-nano holes, micro-nano periodic structures, micro-nano flowers). The sizes of these micro-nano structures span 5 orders of magnitude, making the surface of the processed silicon carbide ceramic material appear black and blue. The water absorption line width is 200 μm and the depth is 60 μm.

[0064] Example 2

[0065] The embodiment of the present invention also provides a method for preparing a silicon carbide ceramic material with strong evaporation performance, comprising the following steps:

[0066] (1) The silicon carbide ceramics used for processing were purchased from Guangzhou Beilong Electronics Co., Ltd. and were made by pressureless sintering. The hardness was 110-120HS and the volume density was >3.10g / cm 3 , the thermal expansion coefficient is 4×10 -6 -4.5×10 -6 / ℃, thermal conductivity of 90-110W / mk, size of 25×75mm, thickness of 1mm. The silicon carbide ceramic sheet was polished to make its surface smooth and flat, and then ultrasonically cleaned for 20 minutes to control the surface morphology after laser processing, and finally fixed on the displacement platform of femtosecond laser processing.

[0067] (2) A femtosecond laser processing experimental platform was built in an ambient air with a temperature of 24°C and a relative humidity of 50%. The femtosecond laser used was from Astrella Corporation in the United States. The laser amplification system generated 83fs pulses with an energy of approximately 7mJ per pulse and a central wavelength of 800nm.

[0068] (3) The silicon carbide ceramic sheet was fixed on an XYZ displacement platform that was precisely controlled by a computer. The distance, speed, and step length of the displacement platform were precisely controlled by a program written in LabVIEW. The femtosecond laser was started to process the surface of the silicon carbide ceramic sheet. The processing parameters were as follows: the laser energy density was 10.8 J / cm 2 , the step length between scanning lines is 120μm, and the scanning speed is 0.2mm / s. The movement of the material is controlled by the displacement platform. After the displacement platform controls the material to process a distance of 50mm, it steps 120μm in the vertical direction until 24mm is processed in the vertical direction, and finally a silicon carbide material with a processing area of ​​50*24mm is obtained. After that, the same laser energy and scanning speed are used to process twice directly below the processing area to obtain a groove water absorption line for regulating the water inflow. The water absorption line width is 200μm and the depth is 60μm. After completing the processing, a three-dimensional laser scanning microscope (VK-X1100) is used to study the structure of the material surface.

[0069] A series of parallel grooves with a depth of 20 μm and a spacing of 120 μm between adjacent grooves are obtained, and the grooves are rich in micro-nano structures (micro-nano holes, micro-nano periodic structures, micro-nano flowers). The size of these micro-nano structures spans 5 orders of magnitude, making the surface of the processed silicon carbide ceramic material appear black and blue. The width of the water absorption line is 200 μm and the depth is 60 μm.

[0070] like Figure 1The 3D image (a) and SEM image (b) of the silicon carbide ceramic material surface are shown. The right side of image (a) is the actual image of the material. The black thin line below the actual image is the water absorption line. Figures (c), (d), and (e) correspond to the peak, valley, and bottom of the groove, respectively. Figures (f), (j), and (h) are local enlarged images of the peak, valley, and bottom of the groove, respectively. Figures (i), (j), and (k) are similar. From the characterization results, it can be seen that the depth of the groove on the ceramic surface after femtosecond laser processing is about 20μm, the step length is about 120μm, and the processing error is about 1um. The rich micro-nano structure in the groove makes the material surface have excellent capillary pumping ability and light absorption ability.

[0071] Example 3

[0072] In view of the fact that solar radiation is the only source of energy input in the evaporation process, it is of great significance to improve the absorption rate of the silicon carbide surface structure to the spectrum. The present invention provides the absorption rate of the silicon carbide surface structure to spectra of different wavelengths, and pays special attention to its absorption performance within the solar spectrum range. At the same time, it is compared with the original silicon carbide material without laser processing. The reflectivity (R) and transmittance (T) of the material were measured in the wavelength range of 200-2500nm using a Perkin-Elmer-lambda950 spectrophotometer. In order to measure the reflectivity of the wet sample, a water droplet was deposited on the sample to form a water film covering the entire surface of the structure. The nanoscale microstructure formed by laser ablation and the increase in the surface oxygen content induce higher light absorption, achieving effective photothermal conversion. The processed wet silicon carbide has a light absorption rate of up to 0.98 (200-2500nm) at 200-2500nm. Figure 2 ), strongly absorbs sunlight and has the potential to become an efficient solar evaporator.

[0073] Example 4

[0074] In order to evaluate the effect of the shape of the air-water interface on the evaporation rate, we conducted a sessile droplet evaporation experiment under the experimental conditions of room temperature 24℃ and humidity 50±2%. A high-speed camera (Phantom VEO 710L, USA) was used to shoot at a rate of 1000 frames / second to record the diffusion and evaporation process of water droplets on the strong evaporation silicon carbide ceramic material prepared in Example 2. The main device of the experiment is a high-precision balance (Zhuo Jing BS1204, China) with a measurement accuracy of 0.00001. The processed hydrophilic silicon carbide material is placed on this balance. A 15μl deionized water droplet is sent to the central area of ​​the material through an injection pump, and a high-speed camera is used to monitor the diffusion of water droplets on the material in real time. The computer connected to the balance prints out the current balance reading every second. The evaporation rate on silicon carbide is calculated by the mass loss per second and the wetted area at the current moment.

[0075] Three-dimensional solar evaporation material evaporation rate test device at room temperature, such as Figure 5 As shown in (a), it includes a high-precision balance, a windshield is built around the high-precision balance, a high-speed camera looking down is placed on the top of the windshield, a high-speed camera looking sideways is placed on the outside of the windshield, an LED lamp is placed in the windshield as a supplementary light source, and an LED can also be set outside the windshield as a supplementary light source; a needle for controlling the volume of liquid is suspended above the tray of the balance, the needle is connected to a syringe, and a computer controls the volume of liquid dripped from the needle by controlling the syringe; the center point of the sample material is placed under the needle; the distance between the sample material and the needle tube is adjusted so that the droplet hanging on the needle just touches the sample material; the deionized water dripped into the needle tube begins to diffuse from the center of the sample, the balance is connected to the computer, and the mass of the sample material and water at each time point is printed in real time. Both the high-speed camera looking down and the high-speed camera looking sideways are connected to the computer. The windshield is used to reduce the influence of air flow on the balance indication, while the high-speed camera looking down is used to monitor the change of the wet area during evaporation, and the use of the LED light source is more conducive to the side-viewing high-speed camera observing the light reflection of different air-water interfaces. The high-speed camera looking down shoots the wet area at a speed of 50 frames per second. The captured images were processed with XARA software to obtain the ratio of the wetted area to the processed area. The ratio was multiplied by the actual processed area to obtain the actual wetted area.

[0076] The method for testing the evaporation rate using the above device comprises the following steps:

[0077] 1) Set the volume of deionized water, turn on the balance printing function, and start recording with a high-speed camera at 50 frames per second;

[0078] 2) Drop a 15 μl droplet into the material, which quickly spreads as a water film on the surface of the material. Wait for the droplet to evaporate completely and stop recording and printing.

[0079] 3) Measure the mass m1 of the droplet that decreases per second, and obtain the projected wetted area s1 at the corresponding time point through image processing;

[0080] 4) The side-view high-speed camera focuses on the material surface when the water drop just drips in, because the water film is the thickest at the location where the water drop drips in. The camera can capture the interface state during the evaporation time, and the captured image is used to visualize the effect of water film thickness on evaporation rate;

[0081] 5) Calculate the evaporation rate at each time point when the silicon carbide ceramic material sample is placed horizontally according to the following formula:

[0082]

[0083] 6) In order to further ensure the accuracy of the experimental results, the same steps were used for measurement 5 times, and the average value of the 5 results was taken.

[0084] In order to evaluate the ability of the material prepared by the present invention to enhance evaporation, the evaporation rate of free water in the container was also measured. The results showed that the evaporation rate on the silicon carbide material was 270 times that of free water. The top-view camera was used to monitor the projected wetted area, and the side-view camera had a high-power microscope lens for optical visualization of the shape of the air-water interface. The mass loss, the spreading shape of the water droplets on the material, and the state of the air-water interface were tracked in real time by a balance and a high-speed camera. Figure 3 In the figure, a and b respectively represent the evaporation rate at each moment during the evaporation of the water film and the evaporation enhancement relative to the evaporation of free water, (a1)-(a9) represent the spreading shape of the water droplets at different moments, and (b1)-(b9) represent the state of the air-water interface at different moments under the high-power optical lens. The evaporation rate changes with time. 0-3s is the thick film state, 4-55s is the thin film state, 56-245s is the ultra-thin film state, and the mass is the same at 246s and 247s, when the material is dry. Since the thickness of the water film changes with the distance at the same time, there is only a wet area in the center of the material in the last few moments. In order to monitor the shape of the air-water interface at all times, the side-view camera is photographed in the center of the material. At 0s, the water droplet is suspended above the material, and the surface of the dry material appears gray. The next second, the water droplet contacts the material and quickly spreads on the material. After 2 seconds, the thick film in the center area spreads into a thin film. It is generally believed that in the pictures taken by the top-down camera, the water surface of the thick film will be higher than the material surface; there are many small bright spots in the water film corresponding to the thin film (the central area of ​​a2); and the ultra-thin film is a black area with very few bright spots (a4). In the top-down camera, the air-water interface shape of the thick film is shown as the water surface covering the material, which is a flat and smooth water film; the air-water interface shape of the thin film is the meniscus formed by water in the groove (b2); as the water in the groove disappears, the water is confined in the microstructure and nanostructure, and the shape of the air-water interface at this time is the ultra-thin film state (b3-b8). At 7s, white rings began to appear at the edge of the wetting area, and snapshot b2 shows that the air-water interface shape at this time is curved in the groove. The white ring of the water film diffusion front becomes clearly visible at 26s, and the meniscus drops to the bottom of the groove. As the water front spreads, the thin film stage (TnWF) ends at about 55s. The evaporation in the TnWF stage is mainly explained by two mechanisms: evaporation in the three-phase (solid-liquid-gas) contact line region and evaporation in the meniscus in the groove. A black ultrathin film (a3) ​​appears at 55 s, and snapshot b3 shows that water is confined to the micron / nanostructure. The micron-scale meniscus appears as a tiny white spot in the top-down snapshot. After a period of evaporation dominated by UnWF, the evaporation rate increases from 9.91 μg cm at 55 s to 1.3 μg cm at 1.5 s. -2 s -1 It increased to 28.68 μg cm at 102 s. -2 s-1 , and then (about 102-210s) the evaporation rate increased by about ten times and began to oscillate. The oscillation of the evaporation rate can be explained by the curvature jitter of the micron / nanoscale meniscus. At 102s, the meniscus of the microstructure became smaller and the area of ​​the outer white ring continued to increase. In the snapshot (b4), it can be seen that the meniscus in the microstructure almost disappeared and many small light spots appeared. The appearance of the small light spots is due to the reflection of the nanoscale water film, which is similar to the reflection of the meniscus in the microgroove. Therefore, at 162s, most of the water was confined in the nanostructure, and the evaporation rate reached 27.25μg cm -2 s -1 . When the material is not completely dry, it should appear darker than the 0s snapshot. The side view snapshot and top view snapshot shown at 7-198s show the material in black, which is in line with expectations. However, at 222-244s, the side view snapshot and top view snapshot show a whiter or brighter color than the completely dry interface. When light encounters an interface with different density, refractive index or material roughness, it will scatter on the surface or inside in different ways. We believe that the phenomenon of the material turning white comes from Rayleigh scattering. Silicon carbide materials are rich in nanoscale structures. During the evaporation of ultra-thin water films, some nanopores contain steam that has not been discharged in time due to rapid evaporation, some contain water vapor mixtures, and some nanopores contain water films with a thickness of several molecules. These structures are comparable to the wavelength of visible light and can scatter all wavelengths in visible light, making the material appear white, just like clouds in the macroscopic world exist in nanostructures. The appearance of this water film brings about super strong evaporation, which is 330 times stronger than the evaporation of the free water surface.

[0085] Example 5

[0086] Using a xenon lamp to simulate sunlight, the evaporation rate of the material was measured at 1sun, 2sun, 3sun, and 4sun light intensities to analyze the evaporation capacity of the material. The solar energy experimental platform was built as follows: Figure 5 (b) as shown:

[0087] Xenon lamp: Beijing Perfect Light, model PLS-SXE300D, spectral range 300-2500μm, light outlet spot diameter 30-63mm, working mode electronic control and optical control, anode heat sink working temperature 76℃, light instability (transient) less than 0.5%.

[0088] Electronic balance: Zhuojing electronic analytical balance produced by Shanghai Zhuojing Company, model BS1204, maximum weighing is 120g, minimum weighing is 0.1mg, weighing pan size is Ф90 (inner diameter), accuracy level: Ⅰ, net weight (approximately): 4.0kg.

[0089] Lens: Focal length is 15mm, used to focus the light beam.

[0090] Rectangular aperture: controls the energy to be incident only on the processing area.

[0091] Material placement method: The lifting platform is on the side of the balance. The material is clamped by the lifting platform and hung in the water container. Foam is placed at the clamping position to prevent heat from the material from being transferred to the device. The water container is sealed.

[0092] like Figure 5 As shown in the figure, the evaporation rate test device of silicon carbide ceramic material under solar energy includes a high-precision balance, a water container, a high-speed camera, a xenon lamp, a filter, a lens and an aperture. The light emitted by the xenon lamp is irradiated onto the surface of the material through the filter, the lens and the aperture; the material is fixed with a THORLABS bracket and placed vertically in the water container, and all surfaces of the water container are sealed to ensure that the water is spread on the material against gravity and evaporates only on the material; the water container and the material are placed on a high-precision balance to record the mass of water evaporated in each time period; changing the input current can accurately simulate the irradiation of sunlight of different intensities. The AM1.5G filter is used to simulate the solar spectrum, and the aperture and lens are used to control the sunlight to irradiate in the processing area. The energy of one sunlight is 1kw m -2 , using an optical power meter to measure the energy reaching the surface of the material, which is 1-4 suns. The lens focuses the collimated light beam so that it irradiates the surface of the material vertically. At the same time, in order to avoid the error of the balance reading caused by the heating of the water in the water container, an aperture is added to the experimental device. The experiment was carried out in a windless environment with a room temperature of 24°C and a relative air humidity of 50%.

[0093] The method for testing the surface evaporation rate of the material under sunlight of the present invention comprises the following steps:

[0094] 1) Place the material vertically in a water container. The capillary force of the material is greater than the gravity. At this time, the water in the water container will be pumped to the surface of the material. When the gravity of the pumped water is balanced with the capillary force, the height of the water film hardly changes. Due to the imbalance caused by evaporation, the height of the water film will change slightly over time, and this change can be ignored macroscopically. Turn on the xenon light source and wait for about 15 minutes. When the light intensity is stable and the vertically spread water film is stable, record the current balance reading m2;

[0095] 2) Wait for a while and record the waiting time t. The waiting time is generally about 20 minutes. The evaporation mass obtained is more accurate. At the same time, record the balance reading m3;

[0096] 3) Calculate the mass loss of water in the water container within the time period, and obtain the projected wet area s1 of the corresponding time period through image processing. The captured image is processed with XARA software to obtain the ratio of the wet area to the processing area. The ratio is multiplied by the actual processing area to obtain the actual wet area s1.

[0097] 4) Calculate the average evaporation rate of silicon carbide ceramic material samples under different light intensities when placed vertically according to the following formula:

[0098]

[0099] 5) In order to further ensure the accuracy of the experimental results, the same steps were used for measurement three times, and the average value of the three results was taken.

[0100] 6) We obtained 10 sets of evaporation data under different solar intensities by two different water pumping methods: through the water absorption line and directly supplying water to the processing area. The results are shown in the figure Figure 4 , Figure 4 a, 4b are optical images of different white film areas, Figure 4 c and Figure 4 d are respectively a comparison chart of the evaporation rate with the patent CN116174926A and a comparison chart of the evaporation rate of different white film areas. The results show that by regulating the water inflow, the water film of the water absorption groove is thinner and the white water film accounts for up to 25%. This processing method provides high evaporation at each sunlight intensity. Under 4 sunlight, the white water film of the ordinary water supply method is only 10%, and the evaporation rate is one quarter of the water absorption groove water supply method. The silicon carbide material of the present invention combined with the water inflow regulation method has excellent evaporation performance.

[0101] Compared with the material in patent CN116174926A, the material of the present invention has richer nanostructure and better evaporation performance, and has a large area of ​​high evaporation white water film that it does not have. The addition of water absorption lines enables the material of the present invention to have the ability to control the thickness of the water film, further optimizing the material in CN116174926A. We compared the evaporation rate of the material of the present invention and the material in patent CN116174926A at different temperatures when the material is placed vertically. The results are as follows Figure 4 c. Under the condition of no wind speed, the material of the present invention with a white film ratio of 25% obtained 34 μg cm at 20°C, 40°C, 60°C, and 80°C respectively. -2 s -1 , 96 μg cm -2 s -1 , 200 μg cm -2 s -1 , 235 μg cm -2 s -1In contrast, the material prepared by patent CN116174926A only obtained 18.16 μg cm at the above four temperatures and a wind speed of 0.5 m / s. -2 s -1 , 22 μg cm -2 s -1 , 34 μg cm -2 s -1 , 44 μg cm -2 s -1 The evaporation rate of the material of the present invention has excellent evaporation performance.

[0102] In the experiment, the water container cannot be completely sealed, but the mass of water evaporated from the free surface is much smaller than the mass of water evaporated from the material surface, so the error caused by incomplete sealing can be ignored. Under one sun intensity, the evaporation rate of water on the material can reach 3.45kg m -2 h -1 Similarly, the evaporation rate of water in copper material modified by femtosecond laser under one sun intensity is only 1.97 kg m -2 h -1 And there is no white water film. In contrast, the processed silicon carbide material has excellent evaporation performance. By processing the balance reading, we found that the mass decreases linearly with time, which means that the mass evaporated in each time period is basically unchanged, indicating that the material has stable evaporation performance. As the solar intensity increases, the evaporation rate of the material increases. This is because the higher solar flux induces more solar heat on the surface of the material, providing faster water evaporation. At 4 suns, the evaporation rate can be as high as 9.64kg m -2 h -1 , providing insights into solutions to freshwater issues.

[0103] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A three-dimensional solar evaporation material, characterized in that: The surface has multiple parallel and continuously distributed grooves with a depth of 20 μm and a spacing of 120 μm between adjacent grooves. The grooves are rich in micro-nano structures with sizes spanning 5 orders of magnitude and also include a water absorption line.

2. A three-dimensional solar evaporation material according to claim 1, characterized in that: The water absorption line is set just below the processing area, with a width of 200 μm and a depth of 60 μm.

3. A method for preparing the three-dimensional solar evaporation material according to claim 1 or 2, characterized in that: The following steps are involved: (1) grinding and cleaning the silicon carbide ceramic sheet, and fixing the silicon carbide ceramic sheet on a displacement platform for femtosecond laser processing; (2) A femtosecond laser is used to process the surface of a silicon carbide ceramic sheet. The material movement is controlled by a displacement platform. The same laser energy and scanning speed are used to process the surface directly below the processing area twice to obtain a water absorption line.

4. The method for preparing a three-dimensional solar evaporation material according to claim 3, characterized in that: The processing parameters of the femtosecond laser are: laser energy density 10.6 J / cm 2 , the step length between scanning lines is 120μm, and the scanning speed is 0.2mm / s.

5. The method for preparing a three-dimensional solar evaporation material according to claim 3 or 4, characterized in that: The processing environment of the femtosecond laser is a temperature of 24° C. and a relative humidity of 50%.

6. The use of the three-dimensional solar evaporation material according to claim 1 or 2, characterized in that: Used to prepare photothermal materials for seawater desalination.

7. The three-dimensional solar evaporation material evaporation rate testing device according to claim 1 or 2 at room temperature, characterized in that: The invention comprises a high-precision balance, a windshield is built around the high-precision balance, a high-speed camera looking down is placed on the top of the windshield, a high-speed camera looking sideways is placed on the outside of the windshield, a needle for controlling the volume of liquid is hung above the tray of the balance, a sample material is placed on the tray of the balance, the center point of the sample material is placed under the needle, and the distance between the sample material and the needle is adjusted so that the droplet hanging on the needle just touches the sample material; the balance is connected to a computer to print the mass of the material and water in real time, and the high-speed camera looking down and the high-speed camera looking sideways are connected to the computer.

8. A method for measuring the evaporation rate of three-dimensional solar evaporation materials at room temperature using the device of claim 7, characterized in that: The following steps are involved: 1) Set the volume of deionized water, turn on the balance printing function, and start recording with a high-speed camera at 50 frames per second; 2) Drop a 15 μl droplet into the material, which quickly spreads as a water film on the surface of the material. Wait for the droplet to evaporate completely and stop recording and printing. 3) Measure the mass m1 of the droplet that decreases per second, and obtain the projected wetted area s1 at the corresponding time point through image processing; 4) The side-view high-speed camera focuses on the material surface when the water drop just drips in, because the water film is the thickest at the location where the water drop drips in. The camera can capture the interface state during the evaporation time, and the captured image is used to visualize the effect of water film thickness on evaporation rate; 5) Calculate the evaporation rate at each time point when the silicon carbide ceramic material sample is placed horizontally according to the formula:

9. The three-dimensional solar evaporation material evaporation rate testing device according to claim 1 or 2 under solar energy, characterized in that: It includes a high-precision balance, a water container, a high-speed camera, a xenon lamp, a filter, a lens and an aperture. The light emitted by the xenon lamp is irradiated onto the surface of the material through the filter, the lens and the aperture. The material is fixed by a fixing device and placed vertically in the water container. The water container and the material are placed on a high-precision balance. The mass of water evaporated in each time period is recorded. The balance is connected to a computer to print the mass of the material and water in real time.

10. A method for measuring the evaporation rate of three-dimensional solar evaporation materials under solar energy using the device of claim 9, characterized in that: The following steps are involved: 1) Place the material vertically in a water container. The capillary force of the material is greater than the gravity. At this time, the water in the water container will be pumped to the surface of the material. When the gravity of the pumped water is balanced with the capillary force, the height of the water film hardly changes. Turn on the xenon light source and wait until the light intensity and the vertically spread water film are stable. Then record the current balance reading m2; 2) Wait for time t and record the balance reading m3; 3) Calculate the mass loss of water in the water container within the time period, obtain the projected wet area s1 of the corresponding time period through image processing, process the captured image with XARA software, obtain the ratio of the wet area to the processing area, multiply the ratio by the actual processing area to obtain the actual wet area s1; 4) Calculate the average evaporation rate of silicon carbide ceramic material samples under different light intensities when placed vertically according to the formula:

Citation Information

Patent Citations

  • Device and method for preparing microstructure on surface of silicon crystal through femtosecond laser filaments

    CN105834589A

  • Laser processing device and method

    CN108115296A

  • Application of Te nanoparticles

    CN110182877A

  • Method and system for measuring evaporation rate of silicon material

    CN115575277A

  • Method and device for continuously and fully electrolyzing seawater by using photo-thermal and electro-catalysis dual-function composite nano carbon film

    CN116005172A

Cited By

  • Silicon carbide ceramic material with super wettability at high temperature, preparation method, application and testing device and method

    CN116174926A