Smearing type grounding resistance reducing agent and preparation method and application thereof

By applying a flocculated mixture of cement, filler, metal powder and HPAM on the surface of the ground electrode, the problems of inconvenient construction, unstable effect and environmental impact of existing grounding resistance reducing agents are solved, and high adhesion and conductivity are achieved. Improves the reliability and environmental friendliness of the grounding system.

CN119049755APending Publication Date: 2024-11-29ZUNYI ZHANLU ELECTRIC CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411182920.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing grounding resistance reducing agents are inconvenient to construct, unstable effects, great environmental impact, difficult maintenance, and difficult to disperse conductive materials evenly under high temperature operations, resulting in unobvious or unstable grounding resistance reduction.

Method used

Using coating grounding resistance reducing agents, including cement, filler, metal powder, sodium chloride and HPAM, a flocculated mixture is formed through specific ratios and treatment steps, the pH value is adjusted and sodium hypochlorite solution is added to form a high adhesion, A moisturizing and conductive solid powder is applied directly to the surface of the ground electrode.

Benefits of technology

It realizes simple and fast construction, adapts to the stable reduction of grounding resistance under different soil conditions, improves the reliability and environmentally friendly characteristics of the grounding system, and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049755A_ABST
    Figure CN119049755A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of physical polymer chemical conductive grounding materials, and provides a smearing type grounding resistance reducing agent and a preparation method and application thereof.The smearing type grounding resistance reducing agent comprises a solid powdery formula and a solvent, and the solid powdery formula specifically comprises, by weight, 20-30 parts of cement, 10-15 parts of filler, 10-20 parts of metal powder, 10-15 parts of sodium chloride and 15-25 parts of HPAM; the solvent is a sodium hypochlorite solution, and the weight part of the solvent is 0.5-1 part; according to the present invention, the special formula is adopted, such that the high adhesion, the high moisture retention and the high conductivity are provided, the coating can be directly coated on the surface of the grounding electrode so as to make the surface grounding resistivity of the grounding electrode be 0.36 ohm per square meter, and the advantages of simple and rapid construction, high adaptability and the like are provided; the smearing type grounding resistance reducing agent has good conductivity and stable chemical properties, can effectively reduce grounding resistance under different soil conditions and improve the reliability of a grounding system, and meanwhile, the resistance reducing agent is made of environment-friendly materials, is environment-friendly and meets the requirement of sustainable development.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of physical polymer chemical conductive grounding materials, and specifically describes a smearable grounding resistance reducing agent and a preparation method and application thereof. Background Art

[0002] In the operation of power systems and communication equipment, the reliability and safety of the grounding system are crucial. The main function of grounding is to provide a safe and reliable low-impedance path to effectively conduct current to the earth when equipment fails, thereby protecting equipment and personal safety. However, many factors such as soil resistivity, environmental humidity, corrosiveness, and the material and installation method of the grounding electrode will affect the effect of grounding;

[0003] Grounding resistance reducer is usually a chemical substance used to improve the contact between the grounding electrode and the soil. It can reduce the grounding resistance and improve the reliability of the grounding system. Existing grounding resistance reducers are mostly in the form of solid powder or granules. When used, they need to be mixed with water and poured into the soil around the grounding electrode. Although this method can reduce the grounding resistance to a certain extent, it still has some shortcomings:

[0004] (1) Inconvenient construction: Solid powder or granular resistance reducing agents need to be mixed with water on site, the proportion is difficult to control, and the mixed slurry is difficult to evenly distribute around the grounding electrode.

[0005] (2) Unstable effect: Due to changes in soil type and humidity, the effect of solid resistance reducers may be affected, resulting in unclear or unstable reduction in ground resistance.

[0006] (3) Environmental impact: Some drag reducing agents may contain chemical components that are harmful to the environment, and long-term use may cause pollution to the soil and groundwater.

[0007] (4) Difficult maintenance: Once there is a problem with the grounding system, it needs to be rebuilt, which is costly and time-consuming.

[0008] In a Chinese patent with publication number CN108258450B, a grounding resistance reducing agent and its preparation method and application are proposed. It discloses that a mesoporous organic silica layer is used as a skeleton, the mesoporous organic silica skeleton is mixed with a conductive material mixture, and the mixture is stirred and shaken to load the conductive material on the mesoporous organic silica skeleton, and then a foaming material is injected to uniformly disperse the conductive material in the foaming material to obtain a grounding resistance reducing agent; however, this installation method requires high-temperature operation, complicated procedures, and inconvenient construction; in a Chinese patent with publication number CN105225769, a grounding grid physical resistance reducing agent for alkaline soil is proposed, which discloses that the resistance reducing agent is prepared by adding conductive fillers, sodium-based bentonite, etc. to a foaming material and then stirring. The foaming material used in this scheme is Acrylic acid-acrylate copolymer system; however, the foaming material is a polymer material, and conductive materials and materials such as sodium-based bentonite are difficult to be evenly dispersed in the foaming system due to external stirring, resulting in uneven distribution of conductive materials and unstable performance of grounding resistance reduction materials; in the Chinese patent with publication number CN104318973B, an acrylic acid-modified bentonite resistance reducing agent is proposed, which uses acrylic acid-modified bentonite to prepare the resistance reducing agent; Patent CN102750999B introduces the use of sodium bicarbonate, sodium carbonate and water to prepare a copper grounding grid resistance reducing agent; however, the conductive material in the above patents is a small molecule salt or a water-soluble non-cross-linked polymer, which is easily lost by rain erosion during application, and is still insufficient in stability, long-term effectiveness and other functions.

[0009] To this end, those skilled in the art have proposed a smearable grounding resistance reducing agent and a preparation method and application thereof. Summary of the invention

[0010] In order to solve the above technical problems, the present invention provides a smearable grounding resistance reducing agent and a preparation method and application thereof to solve the problems mentioned in the background technology.

[0011] According to the first aspect of the present disclosure, a smearable grounding resistance reduction agent is proposed, comprising a solid powder formula and a solvent, wherein the solid powder formula specifically comprises the following components in proportions by weight: 20-30 parts of cement, 10-15 parts of filler, 10-20 parts of metal powder, 10-15 parts of sodium chloride, and 15-25 parts of HPAM; the solvent is a sodium hypochlorite solution, with a weight ratio of 0.5-1 part.

[0012] Preferably, the filler is coal powder or activated carbon powder; the metal powder is 10-50 mesh iron powder or copper powder. Because the smaller the particles and the more evenly dispersed they are, the more conducive they are to forming a conductive network, thereby improving the conductive performance. However, too high a concentration may cause the conductive material to agglomerate in the matrix, which in turn reduces the conductive performance, so 10-20 parts is the preferred ratio;

[0013] Preferably, the weight ratio of the components is: 30 parts of cement, 15 parts of activated carbon powder, 20 parts of iron powder, 13.5 parts of sodium chloride, 21 parts of HPAM, and 0.5 parts of sodium hypochlorite solution.

[0014] According to the second aspect of the present disclosure, a method for preparing a smearable grounding resistance reducing agent is proposed, comprising the following preparation steps:

[0015] S1, mixed powder: 30 parts of cement, 15 parts of activated carbon powder, 20 parts of iron powder, 13.5 parts of sodium chloride and 21 parts of HPAM are mixed evenly to fully mix the components to obtain a uniform drag-reducing powder formula A1;

[0016] S2, hydrolysis reaction: ionize the sodium hypochlorite solution, reaction equation: NaCI0+H20→HCIO+NaOH to decompose into hypochlorous acid solution and NaOH solution, dilute with water in a ratio of 1:5 of hypochlorous acid to obtain a hypochlorous acid diluted solution A2 suitable for the reaction;

[0017] S3. Preparing a flocculent mixture: Mix the mixed powder A1 and water in a ratio of 1:1.5, and stir for 30 minutes to fully dissolve the HPAN to form a flocculent mixture A3.

[0018] S4. Polymerization reaction control: add NaOH solution through A3 to adjust the pH value of the flocculent mixture to 10.5-11, and add the diluted sodium hypochlorite solution and stir rapidly. After stirring for 15-30 seconds, immediately apply it to the required grounding area with a coating thickness of 4 mm.

[0019] Preferably, in the process of adding NaOH to adjust the pH value, NaOH, as a strong base, reacts with the hydrogen ions in the water to neutralize and reduce the H + concentration, increasing the pH value. The neutralization reaction is expressed as: NaOH+H + →Na + +H2O, and adjust the pH value from the initial pH value of the flocculent mixture to the target pH value, calculate the number of moles of NaOH required within the pH change range, and estimate it as: moles NaOH = volume × (target H+-initial H+), where volume is the total volume of the mixture, H + is the molar concentration of hydrogen ions; according to the concentration of NaOH solution, calculate the volume of NaOH solution added: where concentrationNaOH is the concentration of the NaOH solution used.

[0020] Preferably, the NaOH solution is added in batches to control the pH value in the reaction system to avoid excessive adjustment that causes the pH value to exceed the expected range; at the beginning of the reaction, the required amount of NaOH is calculated based on the expected pH value and the initial pH value of the mixture, and 60%-70% of the total amount is added first, so that there is a sufficient alkaline environment when the reaction starts;

[0021] When the reaction is halfway done, i.e., 50% of the total reaction time, the pH value is retested, and based on the test result, the remaining required amount of 30% NaOH solution is added, and stirring is continued while monitoring the pH value;

[0022] When the reaction is nearly complete, i.e., 80%-90% of the total reaction time, the pH value is checked again, and the remaining required amount of 10% NaOH solution is added to reach the final target pH value.

[0023] Preferably, during the polymerization reaction control, the reaction temperature is controlled to be 20-25°C.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention has strong adhesion, moisture retention and conductivity by adopting a special formula. It can be directly applied to the surface of the grounding electrode to make its surface grounding resistivity 0.36 ohms per square meter. It also has the advantages of simple and quick construction and strong adaptability. The smearable grounding resistance reduction agent has good conductivity and stable chemical properties, can effectively reduce the grounding resistance under different soil conditions, and improve the reliability of the grounding system. At the same time, the resistance reduction agent is made of environmentally friendly materials, is environmentally friendly, and meets the requirements of sustainable development. Through this new type of smearable grounding resistance reduction agent, the efficiency and safety of the grounding project can be greatly improved, and the maintenance cost can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention is a flow chart of the preparation method of the smearable grounding resistance reducing agent. DETAILED DESCRIPTION

[0027] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0028] As attached Figure 1 As shown:

[0029] Embodiment 1: The present invention provides a smearable grounding resistance reducing agent and a preparation method and application thereof, including a solid powder formula and a solvent, wherein the solid powder formula specifically includes the following components in proportion by weight:

[0030] (1) 25 parts of cement, 16 parts of filler, 20 parts of metal powder, 13.5 parts of sodium chloride, 25 parts of HPAM, and 0.5 parts of sodium hypochlorite solution.

[0031] (2) 30 parts cement, 16 parts filler, 15 parts metal powder, 13.5 parts sodium chloride, 2 parts HPAM, 0.5 parts sodium hypochlorite solution

[0032] (3) 25 parts cement, 20 parts filler, 20 parts metal powder, 13 parts sodium chloride, 21 parts HPAM, 1 part sodium hypochlorite solution

[0033] (4) 30 parts of cement, 20 parts of filler, 10 parts of metal powder, 14.5 parts of sodium chloride, 25 parts of HPAM, 0.5 parts of sodium hypochlorite solution

[0034] The filler is coal powder and activated carbon powder; the metal powder is 10-50 mesh iron powder or copper powder. Because the smaller the particles and the more evenly dispersed they are, the more conducive they are to forming a conductive network, thereby improving the conductive performance. However, too high a concentration may cause the conductive material to agglomerate in the matrix, which in turn reduces the conductive performance, so 10-20 parts is the preferred ratio.

[0035] From the above, we can see that HPAM, as a thickener and adhesive, helps to improve the adhesion and stability of the resistance reducing agent; coal powder or activated carbon has adsorption properties, and when dissolved with HPAM, it has a water-locking and moisturizing effect, which can increase the contact area between the grounding resistance reducing agent and the soil and improve conductivity; metal powder is used to enhance conductivity; sodium chloride, as an electrolyte, can improve the conductivity of the solution; cement is used to provide structural strength to ensure the durability of the resistance reducing agent in the soil; sodium hypochlorite solution: as an oxidant, it participates in the polymerization reaction and also has a disinfecting effect.

[0036] Embodiment 2: The present invention also provides a method for preparing a smearable grounding resistance reducing agent, comprising the following preparation and reaction steps:

[0037] S1, mixed powder: 30 parts of cement, 15 parts of activated carbon powder, 20 parts of iron powder, 13.5 parts of sodium chloride and 21 parts of HPAM are mixed evenly to fully mix the components to obtain uniform resistance-reducing powder A1;

[0038] S2, hydrolysis reaction: ionize the sodium hypochlorite solution, reaction equation: NaCI0+H20→HCIO+NaOH to decompose into hypochlorous acid solution and NaOH solution. Dilute the hypochlorous acid with water in a ratio of 1:5 to obtain a hypochlorous acid diluted solution A2 suitable for the reaction;

[0039] S3, preparation of flocculent mixture: mixed powder A1 and water in a ratio of 1:1.5, and stirred for 30 minutes to fully dissolve HPAN to form a flocculent mixture A3.

[0040] S4. Polymerization reaction control: add NaOH solution through A3 to adjust the pH value of the flocculent mixture to 10.5-11, control the reaction temperature to 20-25°C, add A2 and stir quickly. After stirring for 15-30 seconds, immediately apply it to the required grounding area with a coating thickness of 4 mm.

[0041] When applied on the ground and cement floor, it increases the flocculation effect to form a gel that locks in moisture and has a better conductive effect.

[0042] When adding NaOH to adjust the pH value, NaOH, as a strong base, reacts with the hydrogen ions in the water to neutralize and reduce the H + concentration, increasing the pH value. The neutralization reaction is expressed as: NaOH+H + →Na + +H2O, and adjust the pH value from the initial pH value of the flocculent mixture to the target pH value, and calculate the number of moles of NaOH required within the pH change range, which can be estimated as: moles NaOH = volume × (target H + - Initial H + ), where volume is the total volume of the mixture, H + is the molar concentration of hydrogen ions; according to the concentration of NaOH solution, calculate the volume of NaOH solution added: Wherein, concentration NaOH is the concentration of the NaOH solution used. By accurately measuring the initial pH value of the mixture, clarifying the adjustment target and the pH value to be achieved, and combining the above steps, the amount of NaOH required to adjust the flocculent mixture to alkaline conditions can be effectively calculated to ensure that the polymerization reaction between HPAM and sodium hypochlorite occurs smoothly.

[0043] The NaOH solution is added in batches to control the pH value in the reaction system to avoid excessive adjustment that causes the pH value to exceed the expected range; at the beginning of the reaction, the required amount of NaOH is calculated based on the expected pH value and the initial pH value of the mixture, and 60%-70% of the total amount is added first, so that there is a sufficient alkaline environment when the reaction starts;

[0044] When the reaction is halfway done, i.e., 50% of the total reaction time, the pH value is retested, and based on the test result, the remaining required amount of 30% NaOH solution is added, and stirring is continued while monitoring the pH value;

[0045] When the reaction is nearly complete, i.e., 80%-90% of the total reaction time, the pH value is checked again, and the remaining required amount of 10% NaOH solution is added to reach the final target pH value.

[0046] In the polymerization reaction control, the pH value of the reaction system can be effectively controlled and the polymerization reaction conditions can be optimized by gradually adjusting and adding NaOH solution in batches.

[0047] Application experiment example: The conventional graphite resistance reducing agent and the coating type ground resistance reducing agent of the present invention were used to make an experimental comparison on a square meter of floor tiles with a floor moisture content of 8.5, as shown in the following table:

[0048]

[0049]

[0050] Conventional graphite drag reducers are mainly composed of fine graphite and other conductive materials, with an adhesion of about 85%. They can only cling to the ground body at a certain relative humidity, but compared with the drag reducer of the present invention, their adhesion performance is obviously insufficient. In terms of weather resistance, conventional graphite drag reducers are about 70%, which is more susceptible to environmental factors, and their performance may decline under extreme climatic conditions. The weather resistance of the present invention is better than other drag reducers on the ground, rock, cement ground, etc. with a humidity of more than 10% (Note: the effect will be better if applied to cement surfaces and ground).

[0051] There are many factors that affect the human body's ability to withstand electric shock, including:

[0052] Current size: The larger the current, the greater the harm to the human body;

[0053] Type of current: alternating current is more harmful to the human body than direct current;

[0054] Power-on time: The longer the power-on time, the greater the harm to the human body;

[0055] Current path: The path that current takes through the human body is different, causing different degrees of damage to organs;

[0056] Human condition: The age, gender, health status, contact area, etc. of the human body will affect the ability to withstand leakage. Generally speaking, the sensitivity of the human body to electric current is as follows:

[0057] Below 1mA: The human body generally has no feeling;

[0058] 1-10mA: fingers feel numb;

[0059] 10-25mA: Muscle rigidity, difficult to get rid of electric shock;

[0060] 25-50mA: breathing difficulties;

[0061] 50-100mA: Heart fibrillation, possible death;

[0062] Above 100mA: The heart stops beating and death occurs quickly.

[0063] In summary, the invention can be used to introduce current to the ground and the principle of leakage protection to form a complete relay protection system. It can effectively prevent leakage and electric shock of household appliances, making people and property safer and more secure; it has a wide range of uses and can be installed and applied separately to high-rise user families; it replaces the traditional use of ground wires. When used in home decoration, the invention does not require the installation of ground wires, and the construction is more convenient, thus saving time and cost.

[0064] Importantly, it should be noted that the construction and arrangement of the present application shown in a plurality of different exemplary embodiments are only exemplary. Although only a few embodiments are described in detail in this disclosure, it should be readily understood by those who refer to this disclosure that many modifications are possible (e.g., the size, scale, structure, shape and proportion of various elements, as well as parameter values ​​(e.g., temperature, pressure, etc.), mounting arrangements, use of materials, color, directional changes, etc.) without substantially departing from the novel teachings and advantages of the subject matter described in the application. For example, the element shown as integrally formed can be composed of multiple parts or elements, the position of the element can be inverted or otherwise changed, and the nature or number or position of the discrete element can be changed or changed. Therefore, all such modifications are intended to be included in the scope of the present invention. The order or sequence of any process or method steps can be changed or reordered according to alternative embodiments. In the claims, any "device plus function" clause is intended to cover the structure described herein that performs the function, and is not only structurally equivalent but also equivalent structure. Without departing from the scope of the present invention, other replacements, modifications, changes and omissions can be made in the design, operating conditions and arrangement of the exemplary embodiments. Therefore, the invention is not limited to a specific embodiment, but extends to several modifications still falling within the scope of the appended claims.

[0065] Additionally, in order to provide a concise description of exemplary embodiments, all features of an actual embodiment (ie, those features that are not relevant to the best mode presently contemplated for carrying out the invention or those that are not relevant to implementing the invention) may not be described.

[0066] It should be understood that in the development of any actual implementation, as in any engineering or design project, numerous implementation-specific decisions may be made. Such a development effort may be complex and time-consuming, but for those of ordinary skill having the benefit of this disclosure, without undue experimentation, the development effort will be a routine task of design, fabrication, and production.

[0067] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A smearable grounding resistance reducing agent, characterized in that: The invention comprises a solid powder formula and a solvent, wherein the solid powder formula specifically comprises the following components in proportion by weight: 20-30 parts of cement, 10-15 parts of filler, 10-20 parts of metal powder, 10-15 parts of sodium chloride and 15-25 parts of HPAM; the solvent is a sodium hypochlorite solution in a proportion of 0.5-1 parts by weight.

2. A smearable grounding resistance reducing agent as claimed in claim 1, characterized in that: The filler is coal powder or activated carbon powder; the metal powder is iron powder or copper powder.

3. A smearable grounding resistance reducing agent as claimed in claim 1, characterized in that: The weight ratio of the components is: 30 parts of cement, 15 parts of activated carbon powder, 20 parts of iron powder, 13.5 parts of sodium chloride, 21 parts of HPAM, and 0.5 parts of sodium hypochlorite solution.

4. A method for preparing a smearable grounding resistance reducing agent, using the smearable grounding resistance reducing agent according to any one of claims 1 to 3, characterized in that: The method comprises the following preparation steps: S1, mixed powder: 30 parts of cement, 15 parts of activated carbon powder, 20 parts of iron powder, 13.5 parts of sodium chloride and 21 parts of HPAM are mixed evenly to fully mix the components to obtain uniform resistance-reducing powder A1; S2, hydrolysis reaction: ionize the sodium hypochlorite solution, reaction equation: NaCI0+H20→HCIO+NaOH to decompose into hypochlorous acid solution and NaOH solution, dilute with water in a ratio of 1:5 of hypochlorous acid to obtain a hypochlorous acid diluted solution A2 suitable for the reaction; S3, preparing a flocculent mixture: mixing the mixed powder A1 with water in a ratio of 1:1.5, and stirring for 30 minutes to fully dissolve the HPAN to form a flocculent mixture A3; S4. Polymerization reaction control: add NaOH solution through A3 to adjust the pH value of the flocculent mixture to 10.5-11, and add A2 and stir quickly. After stirring for 15-30 seconds, immediately apply it to the required grounding area with a coating thickness of 4 mm.

5. A method for preparing a smearable grounding resistance reducing agent as claimed in claim 4, characterized in that: In the process of adding NaOH to adjust the pH value, NaOH, as a strong base, reacts with the hydrogen ions in the water to neutralize and reduce the H + concentration, increasing the pH value. The neutralization reaction is expressed as: NaOH+H + →Na + +H2O, and adjust the pH value from the initial pH value of the flocculent mixture to the target pH value, and calculate the number of moles of NaOH required within the pH change range, which can be estimated as: moles NaOH = volume × (target H + - Initial H + ), where volume is the total volume of the mixture, H + is the molar concentration of hydrogen ions; according to the concentration of NaOH solution, calculate the volume of NaOH solution added: where concentrationNaOH is the concentration of the NaOH solution used.

6. A method for preparing a smearable grounding resistance reducing agent as claimed in claim 5, characterized in that: The NaOH solution is added in batches to control the pH value in the reaction system to avoid excessive adjustment that causes the pH value to exceed the expected range; at the beginning of the reaction, the required amount of NaOH is calculated based on the expected pH value and the initial pH value of the mixture, and 60%-70% of the total amount is added first to ensure a sufficient alkaline environment when the reaction starts; When the reaction is halfway done, i.e., 50% of the total reaction time, the pH value is retested, and based on the test result, the remaining required amount of 30% NaOH solution is added, and stirring is continued while monitoring the pH value; When the reaction is nearly complete, i.e., 80%-90% of the total reaction time, the pH value is checked again, and the remaining required amount of 10% NaOH solution is added to reach the final target pH value.

7. A smearable grounding resistance reducing agent and a preparation method thereof as claimed in claim 4, characterized in that: During the polymerization reaction control, the reaction temperature is controlled at 20-25°C.

Citation Information

Patent Citations

  • Anti-corrosion resistance reduction agent for copper ground grid

    CN102750999B

  • A kind of acrylic acid modified bentonite drag reducing agent

    CN104318973B

  • A grounding resistance reducing agent, its preparation method, and its application

    CN108258450B