Color-changing filter material for removing ammonia gas and hydrogen sulfide and preparation method of color-changing filter material

By mixing adsorbent substrate and additives with copper sulfate solution, color change caused by ammonia and hydrogen sulfide is solved, and the problem of difficult to intuitively judge material performance in the prior art is achieved efficiently removing ammonia and hydrogen sulfide effect, suitable for industrial applications.

CN119056192APending Publication Date: 2024-12-03SHANXI NABOCO NEW MATERIAL TECHNOLOGY CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310600284.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When removing ammonia and hydrogen sulfide in the prior art, it is difficult to intuitively judge the changes in material properties through the naked eye, resulting in inconvenient use and poor removal effect.

Method used

The adsorbed substrate and additives are added to copper sulfate solution, and then pulverized, emulsified, homogenized and mixed to form a coating slurry, coated on the porous embryo, and color-changing filter material is prepared by purging and drying. The reaction of copper sulfate with ammonia and hydrogen sulfide causes color changes, and the performance of the material is intuitively judged.

Benefits of technology

It achieves efficient removal of ammonia and hydrogen sulfide at room temperature. The color changes can intuitively judge the performance of the filter material. The removal rate is generally as high as 99% or above. It is simple to operate, cheap and easy to obtain, and is suitable for industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056192A_ABST
    Figure CN119056192A_ABST
Patent Text Reader

Abstract

The invention provides a color-changing filter material for removing ammonia gas and hydrogen sulfide and a preparation method of the color-changing filter material, and belongs to the technical field of air purification. A preparation method of a color-changing filter material for removing ammonia gas and hydrogen sulfide comprises the following steps: sequentially adding an adsorption base material and an auxiliary agent into a copper sulfate solution, and then crushing, emulsifying, homogenizing and mixing by using a colloid mill to obtain coating slurry; and coating a porous blank with the coating slurry, and then sequentially blowing and drying to obtain the porous ceramic. The color-changing filter material for removing ammonia gas and hydrogen sulfide, provided by the invention, is prepared by the preparation method. The color-changing filter material provided by the invention can efficiently remove ammonia gas and hydrogen sulfide gas at the same time through the synergistic effect of adsorption and complexation in a normal-temperature environment, changes in color in the process, can judge the change of material performance through visual color change with naked eyes, greatly improves the use convenience of the filter material, and is simple in preparation method and low in cost. Cost is low, and popularization and use are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of air purification, and in particular relates to a color-changing filter material for removing ammonia and hydrogen sulfide and a preparation method thereof. Background Art

[0002] The modern independent and enclosed home environment has improved people's living convenience and living experience. At the same time, various odors generated indoors are more likely to gather and difficult to dissipate in time, causing discomfort to residents. Common symptoms include nausea, headache, loss of appetite, olfactory disorders, insomnia and even emotional instability. In addition, indoor odor pollution has a persistent and long-term impact on human health.

[0003] At present, the treatment schemes for amine and sulfur-based malignant gases at home and abroad are mainly focused on adsorption substrates. For example, patent CN105268399B discloses a preparation method of a room-temperature ammonia high-efficiency treatment material and its use method. A room-temperature ammonia high-efficiency treatment material is prepared by using a porous adsorption substrate as a carrier, aluminum chloride, aluminum sol or metaaluminate, zirconium chloride or zirconium oxychloride as a mixed modifier, and sulfuric acid, hydrochloric acid, nitric acid, boric acid or phosphoric acid as a surface treatment agent. However, the room-temperature ammonia high-efficiency treatment material does not have obvious changes that can be visually seen during the purification of ammonia, so it is difficult to judge the changes in product performance during indoor application. Patent CN113058574B discloses a preparation method of an amine-functionalized hydrogen sulfide porous polymer adsorbent. Using an amine-functionalized hydrogen sulfide porous polymer as an adsorbent, efficient adsorption of hydrogen sulfide is achieved, but the adsorbent material cannot visually judge the changes in material performance during use, which brings great inconvenience to the use process.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a color-changing filter material for removing ammonia and hydrogen sulfide and a preparation method thereof, so as to solve the above-mentioned problems.

[0006] In order to achieve the above objectives, the present invention particularly adopts the following technical solutions:

[0007] A method for preparing a color-changing filter material for removing ammonia and hydrogen sulfide, comprising: adding an adsorption substrate and an auxiliary agent to a copper sulfate solution in sequence, and then using a colloid mill to crush, emulsify, homogenize, and mix to obtain a coating slurry;

[0008] The coating slurry is coated on the porous embryo body, and then purged and dried in sequence to obtain the result.

[0009] In order to improve the loading effect of the coating slurry on the embryo, the porous embryo can be coated by dipping it in the coating slurry, wherein the dipping time is preferably 1-2 minutes. The coating slurry is immersed in the porous embryo, and the entire porous embryo can be quickly and completely soaked. If the dipping time is too long, the slurry will block the pores.

[0010] Optionally, the adsorption substrate includes any one or more of high-silicon molecular sieve, activated alumina, and silicon dioxide.

[0011] Optionally, the auxiliary agent includes a binder, a defoamer, and a dispersant; the mass fraction of the binder is 5-10%; the mass fraction of the defoamer is 0.1-1%; and the mass fraction of the dispersant is 0.1-2%.

[0012] Optionally, the copper sulfate solution is obtained by dissolving copper sulfate pentahydrate solid in water; the mass fraction of the copper sulfate solution is 10-20%.

[0013] After repeated experimental verification, as the mass fraction of copper sulfate pentahydrate increases, the prepared color-changing filter material shows a performance curve of first increasing and then stabilizing the removal performance of ammonia and hydrogen sulfide. A mass fraction that is too low (less than 10%) will result in a poor effect of the color-changing filter material in removing ammonia and hydrogen sulfide; the mass fraction of copper sulfate pentahydrate is too high, because at room temperature, the solubility of copper sulfate pentahydrate is about 20.7g / 100g water. If the mass fraction is higher than 20%, part of the copper sulfate pentahydrate will be dissolved in water and part will not be dissolved in water. Therefore, only the copper sulfate pentahydrate dissolved in water will eventually play a role in removing ammonia and hydrogen sulfide, resulting in a waste of copper sulfate pentahydrate. Therefore, the preferred range of the mass fraction of copper sulfate pentahydrate is 10-20%. Optionally, the mass ratio of the adsorption substrate to the copper sulfate pentahydrate is 1:0.4-1.

[0014] Through experimental verification, the color-changing filter materials prepared according to different mass ratios of the adsorption substrate and copper sulfate pentahydrate were compared in their removal performance for ammonia and hydrogen sulfide. The results showed that when the mass of copper sulfate pentahydrate used was less than 0.4 times the mass of the adsorption substrate, the effect of the color-changing filter material on removing ammonia and hydrogen sulfide was poor; when the mass of copper sulfate pentahydrate used was higher than 1 times the mass of the adsorption substrate, the performance of the color-changing filter material on removing ammonia and hydrogen sulfide did not increase significantly; however, as the amount of copper sulfate pentahydrate used increased, the cost increased. Therefore, considering the material performance and cost control, the preferred range of the mass ratio of the adsorption substrate to copper sulfate pentahydrate was selected as 1:0.4-1.

[0015] Optionally, the porous embryo body includes any one of corrugated, ceramic, aluminum honeycomb or paper honeycomb; the wave height of the porous embryo body is selected from any value of 1.6mm, 1.8mm, 2.0mm; the wavelength of the porous embryo body is selected from any value of 3.2mm, 3.6mm, 4.0mm. By optimizing the parameters of the embryo body, the specific surface area of ​​the embryo body is controlled, and the coating amount of the filter material is further adjusted.

[0016] Optionally, the coating temperature is 30-50°C.

[0017] Optionally, the preparation method further comprises: before the coating, pre-treating the coating slurry;

[0018] The pretreatment includes: freezing the coating slurry for 8-10 hours, then heating, thawing the coating slurry at 5-10°C / min and heating it to 80-100°C, keeping it warm for 30-60 minutes, and then cooling it to 30-50°C at 1-5°C / min under stirring. The pretreatment further disperses and activates the active ingredients of the coating slurry, which is beneficial to improving the effect of subsequent coating, making the loading rate of the active ingredients higher and the loading more uniform.

[0019] The present invention adopts a material with high specific surface area and low wind resistance as the embryo, which greatly increases the specific surface area and reduces the wind resistance during use, is conducive to the full contact reaction between the effective ingredients of the coating slurry and ammonia and hydrogen sulfide substances, and improves the purification efficiency per unit time.

[0020] A color-changing filter material for removing ammonia and hydrogen sulfide is prepared by the preparation method.

[0021] Optionally, the initial color of the color-changing filter material is light blue, and during the process of removing ammonia or hydrogen sulfide, the color changes to dark blue or dark brown.

[0022] The color-changing filter material provided by the present invention has an initial color of light blue. When it comes into contact with ammonia and hydrogen sulfide gas, the color changes significantly. After the reaction with ammonia, the filter element gradually changes from light blue to dark blue, and after the reaction with hydrogen sulfide, the filter element gradually changes from light blue to dark brown. This is because the following reactions occur:

[0023] CuSO 4 (Light blue)+4NH 3 →[Cu(NH 3 ) 4 ]SO 4 (dark blue);

[0024] [Cu(NH 3 ) 4 ] 2+ +3H 2S→CuS(dark brown)+4NH 4 + +2HS - ;

[0025] CuSO 4 (Light blue)+H 2 S→CuS (dark brown)+H 2 SO 4 ;

[0026] During use, the change in material performance can be judged by the visual color change to determine whether the filter material needs to be replaced, making the use of the filter material more convenient.

[0027] Beneficial effects of the present invention:

[0028] The preparation method provided by the invention has cheap and readily available raw materials, mild and controllable conditions, simple operation, and is convenient for industrial promotion and use.

[0029] The color-changing filter material provided by the present invention can efficiently remove ammonia and hydrogen sulfide gases at the same time through the synergistic effect of adsorption and complexation at room temperature. During use, the color will change with the reaction with ammonia and hydrogen sulfide. Before contacting ammonia and hydrogen sulfide, the filter material appears light blue due to the presence of copper sulfate. After reacting with ammonia, the filter element gradually changes from light blue to dark blue. After reacting with hydrogen sulfide, the filter element gradually changes from light blue to dark brown, which overcomes the problem that the changes in material properties cannot be visually judged by the naked eye during use of the filter material in the prior art and the lack of convenience in use. And the removal effect of ammonia and hydrogen sulfide is better, and the one-hour removal rate is generally as high as 99% or more. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is the initial appearance of the color-changing filter material provided in the embodiment;

[0032] Figure 2 This is a diagram showing the appearance of the color-changing filter material provided in the embodiment after ammonia is removed;

[0033] Figure 3 This is the appearance of the color-changing filter material provided in the embodiment after removing hydrogen sulfide. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] According to the preparation method provided by the present invention, a color-changing filter material for removing ammonia and hydrogen sulfide is prepared, and the specific steps are as follows:

[0037] S1. A high-silicon molecular sieve with a particle size of 350 mesh was selected as the adsorption substrate. The specific surface area was 800m 2 / g, wherein the small mesopores account for more than 75%, and the mass ratio of high silicon molecular sieve to copper sulfate pentahydrate is 1:0.6, and the high silicon molecular sieve is put into a copper sulfate solution with a mass fraction of 10%;

[0038] S2, further adding 1% by mass of a dispersant, 0.5% by mass of a defoamer, and 5% by mass of a binder to the system obtained in S1, and crushing, emulsifying, homogenizing, and mixing the mixture using a colloid mill to obtain a homogeneous coating slurry;

[0039] S3. Coat the coating slurry obtained in step S2 on a corrugated porous body with a wave height of 1.6 mm and a wavelength of 3.2 mm, and then blow and dry to obtain a light blue filter material, i.e., a color-changing filter material for removing ammonia and hydrogen sulfide.

[0040] Example 2

[0041] According to the preparation method provided by the present invention, a color-changing filter material for removing ammonia and hydrogen sulfide is prepared, and the specific steps are as follows:

[0042] S1. A high-silicon molecular sieve with a particle size of 350 mesh was selected as the adsorption substrate. The specific surface area was 800m 2 / g, wherein the small mesopores account for more than 75%, and the mass ratio of high silicon molecular sieve to copper sulfate pentahydrate is 1:0.6, and the high silicon molecular sieve is put into a copper sulfate solution with a mass fraction of 15%;

[0043] S2, further adding 1% by mass of a dispersant, 0.5% by mass of a defoamer, and 5% by mass of a binder to the system obtained in S1, and crushing, emulsifying, homogenizing, and mixing the mixture using a colloid mill to obtain a homogeneous coating slurry;

[0044] S3. Coat the coating slurry obtained in step S2 on a corrugated porous body with a wave height of 1.6 mm and a wavelength of 3.2 mm, and then blow and dry to obtain a light blue filter material, i.e., a color-changing filter material for removing ammonia and hydrogen sulfide.

[0045] Example 3

[0046] According to the preparation method provided by the present invention, a color-changing filter material for removing ammonia and hydrogen sulfide is prepared, and the specific steps are as follows:

[0047] S1. A high-silicon molecular sieve with a particle size of 350 mesh was selected as the adsorption substrate. The specific surface area was 800m 2 / g, wherein the small mesopores account for more than 75%, and the mass ratio of high silicon molecular sieve to copper sulfate pentahydrate is 1:0.6, and the high silicon molecular sieve is put into a copper sulfate solution with a mass fraction of 20%;

[0048] S2, further adding 1% by mass of a dispersant, 0.5% by mass of a defoamer, and 5% by mass of a binder to the system obtained in S1, and crushing, emulsifying, homogenizing, and mixing the mixture using a colloid mill to obtain a homogeneous coating slurry;

[0049] S3. Coat the coating slurry obtained in step S2 on a corrugated porous body with a wave height of 1.6 mm and a wavelength of 3.2 mm, and then blow and dry to obtain a light blue filter material, i.e., a color-changing filter material for removing ammonia and hydrogen sulfide.

[0050] Example 4

[0051] According to the preparation method provided by the present invention, a color-changing filter material for removing ammonia and hydrogen sulfide is prepared, and the specific steps are as follows:

[0052] S1. A high-silicon molecular sieve with a particle size of 350 mesh was selected as the adsorption substrate. The specific surface area was 800m 2 / g, wherein the small mesopores account for more than 75%, and the mass ratio of high silicon molecular sieve to copper sulfate pentahydrate is 1:0.6, and the high silicon molecular sieve is put into a copper sulfate solution with a mass fraction of 10%;

[0053] S2, further adding 1% by mass of a dispersant, 0.5% by mass of a defoamer, and 5% by mass of a binder to the system obtained in S1, and crushing, emulsifying, homogenizing, and mixing the mixture using a colloid mill to obtain a homogeneous coating slurry;

[0054] S3, freezing the coating slurry obtained in step S2 for 10 hours, then heating it, thawing it at 5°C / min and raising the temperature to 90°C, keeping it warm for 50 minutes, and then lowering the temperature to 50°C at 2°C / min under stirring;

[0055] S4, coating the coating slurry obtained in step S3 on a corrugated porous body with a wave height of 1.6 mm and a wavelength of 3.2 mm, and then blowing and drying to obtain a light blue filter material, i.e., a color-changing filter material for removing ammonia and hydrogen sulfide.

[0056] Comparative Example 1

[0057] According to the preparation method provided by the present invention, a color-changing filter material for removing ammonia and hydrogen sulfide is prepared, and the specific steps are as follows:

[0058] S1. A high-silicon molecular sieve with a particle size of 350 mesh was selected as the adsorption substrate. The specific surface area was 800m 2 / g, wherein the small mesopores account for more than 75%, and the mass ratio of high silicon molecular sieve to copper sulfate pentahydrate is 1:0.3, and the high silicon molecular sieve is put into a copper sulfate solution with a mass fraction of 10%;

[0059] S2, further adding 1% by mass of a dispersant, 0.5% by mass of a defoamer, and 5% by mass of a binder to the system obtained in S1, and crushing, emulsifying, homogenizing, and mixing the mixture using a colloid mill to obtain a homogeneous coating slurry;

[0060] S3. Coat the coating slurry obtained in step S2 on a corrugated porous body with a wave height of 1.6 mm and a wavelength of 3.2 mm, and then blow and dry to obtain a light blue filter material, i.e., a color-changing filter material for removing ammonia and hydrogen sulfide.

[0061] Comparative Example 2

[0062] According to the preparation method provided by the present invention, a color-changing filter material for removing ammonia and hydrogen sulfide is prepared, and the specific steps are as follows:

[0063] S1. A high-silicon molecular sieve with a particle size of 350 mesh was selected as the adsorption substrate. The specific surface area was 800m 2 / g, wherein the small mesopores account for more than 75%, and the mass ratio of high silicon molecular sieve to copper sulfate pentahydrate is 1:1.2, and the high silicon molecular sieve is put into a copper sulfate solution with a mass fraction of 10%;

[0064] S2, further adding 1% by mass of a dispersant, 0.5% by mass of a defoamer, and 5% by mass of a binder to the system obtained in S1, and crushing, emulsifying, homogenizing, and mixing the mixture using a colloid mill to obtain a homogeneous coating slurry;

[0065] S3. Coat the coating slurry obtained in step S2 on a corrugated porous body with a wave height of 1.6 mm and a wavelength of 3.2 mm, and then blow and dry to obtain a light blue filter material, i.e., a color-changing filter material for removing ammonia and hydrogen sulfide.

[0066] Performance Test:

[0067] Test conditions: at 30m 3 In the experimental chamber, the color-changing filter material is 350*250*10mm, and the air volume of the purifier is 400m 3 / h, the color-changing filter materials prepared in Examples 1-4 and Comparative Examples 1-2 were used to test ammonia and hydrogen sulfide respectively.

[0068] First, through naked eye observation, the color-changing filter material provided by the embodiment of the present invention is initially light blue. Figure 1 As shown in the figure, during the test of removing ammonia, the color of the filter material gradually changed from light blue before the experiment to dark blue. Figure 2 As shown in the figure, during the test of removing hydrogen sulfide, the color-changing filter material gradually changed from light blue before the experiment to dark brown. Figure 3 The color development and color change process of the filter material during the removal process is clear and can be judged visually with the naked eye.

[0069] The performance results for the removal of ammonia and hydrogen sulfide are shown in Table 1 below.

[0070] Table 1. Test results of removal performance of color-changing filter materials prepared in Examples 1-4 and Comparative Examples 1-2

[0071]

[0072] As can be seen from Table 1, the filter material provided by the present invention has a better removal effect on ammonia and hydrogen sulfide, and the one-hour removal rate is generally as high as 99% or more.

[0073] It can be seen from Examples 1 and 4 that, under the same other conditions, pretreatment of the coating slurry can significantly improve the dispersibility of the active components in the slurry, and the more evenly dispersed slurry can be coated on the porous embryo body. The filter material performance obtained is also better, showing a higher removal rate of ammonia and hydrogen sulfide.

[0074] By comparing Example 1 and Comparative Example 1, it can be seen that, under the same conditions, only the mass ratio of high silicon molecular sieve to copper sulfate pentahydrate is slightly different, and the performance of the filter material obtained shows great differences. Obviously, under the preferred ratio conditions provided by the present invention, the one-hour removal rate of ammonia and hydrogen sulfide by the filter material is significantly higher than that of Comparative Example 1.

[0075] By comparing Example 1 and Comparative Example 2, it can be seen that when the amount of copper sulfate pentahydrate is much higher than the preferred range of the present invention, the production cost is greatly increased, but the comprehensive performance of the filter material obtained is not significantly improved.

[0076] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.

Claims

1. A method for preparing a color-changing filter material for removing ammonia and hydrogen sulfide, characterized in that: include: The adsorption substrate and the auxiliary agent are sequentially added into the copper sulfate solution, and then crushed, emulsified, homogenized and mixed using a colloid mill to obtain a coating slurry; The coating slurry is coated on the porous embryo body, and then purged and dried in sequence to obtain the result.

2. The preparation method according to claim 1, characterized in that: The adsorption substrate includes any one or more of high-silicon molecular sieve, activated alumina, and silicon dioxide.

3. The preparation method according to claim 1, characterized in that: The auxiliary agents include binders, defoamers and dispersants; The mass fraction of the binder is 5-10%; The mass fraction of the defoamer is 0.1-1%; The mass fraction of the dispersant is 0.1-2%.

4. The preparation method according to claim 1, characterized in that: The copper sulfate solution is obtained by dissolving copper sulfate pentahydrate solid in water; The mass fraction of the copper sulfate solution is 10-20%.

5. The preparation method according to claim 4, characterized in that: The mass ratio of the adsorption substrate to the copper sulfate pentahydrate is 1:0.4-1.

6. The preparation method according to claim 1, characterized in that: The porous embryo body comprises any one of corrugated, ceramic, aluminum honeycomb or paper honeycomb; The wave height of the porous embryo body is selected from any value among 1.6 mm, 1.8 mm, and 2.0 mm; The wavelength of the porous embryo body is selected from any value among 3.2 mm, 3.6 mm and 4.0 mm.

7. The preparation method according to claim 1, characterized in that: The coating temperature is 30-50°C.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method further comprises: before the coating, pre-treating the coating slurry; The pretreatment comprises: freezing the coating slurry for 8-10 hours, then heating, thawing the coating slurry at 5-10°C / min and heating it to 80-100°C, keeping it warm for 30-60 minutes, and then cooling it to 30-50°C at 1-5°C / min under stirring.

9. A color-changing filter material for removing ammonia and hydrogen sulfide, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.

10. The color-changing filter material according to claim 9, characterized in that: The initial color of the color-changing filter material is light blue, and during the process of removing ammonia or hydrogen sulfide, the color changes to dark blue or dark brown.

Citation Information

Cited By

  • Air purification material for removing alkaline pollutants in air as well as preparation method and application of air purification material

    CN120754831A

  • Air purification material for removing alkaline contaminants in air and preparation method and application thereof

    CN120754831B