Biomass-based composite aerogel as well as preparation method and application thereof

By generating CdS@UiO-66-NH2 photocatalytic heterojunction on cellulose nanofibers/chitosan/montmorillonite aerogels in situ, the problem of single function and difficulty in reuse in the prior art is solved, and the problem of single function and difficult to reuse is achieved. It provides a multifunctional green wastewater treatment method by efficient adsorption and photocatalytic degradation of heavy metals and dyes.

CN119056356APending Publication Date: 2024-12-03SHANGHAI INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411172979.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

There is a lack of multifunctional biomass-based composite aerogels that can be used for heavy metal and dye treatment in the prior art, and the existing materials have single functions, poor mechanical properties, low treatment efficiency, difficult to reuse, and there is a risk of secondary pollution.

Method used

Cellulose nanofiber/chitosan/montmorillonite aerogel is used as the matrix to generate CdS@UiO-66-NH2 photocatalytic heterojunction in situ to achieve adsorption of heavy metal ions and photocatalytic degradation of dyes, combined with adsorption The synergy with photocatalysis improves the reusability of the material.

Benefits of technology

It realizes efficient adsorption and photocatalytic degradation of heavy metal ions and dyes, improves the mechanical properties and reusability of the materials, and provides a green and efficient multifunctional wastewater treatment method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056356A_ABST
    Figure CN119056356A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aerogel preparation, and particularly relates to biomass-based composite aerogel as well as a preparation method and application thereof. The preparation method of the biomass-based composite aerogel comprises the following steps: (1) sequentially adding cellulose nanofibers, chitosan, montmorillonite nanosheets and deionized water into an acetic acid aqueous solution, uniformly mixing, and freeze-drying to obtain a cellulose nanofiber / chitosan / montmorillonite (CCM) aerogel matrix material; (2) regulating and controlling the MOF material UiO-66-NH2 to carry out in-situ generation and uniform loading on the prepared CCM matrix material, so as to obtain UiO-66-NH2 / CCM aerogel; and (3) soaking the UiO-66-NH2 / CCM aerogel in a cadmium acetate aqueous solution, adding a sulfide under a heating condition, and further treating to obtain CdS-coated UiO-66-NH2 / CCM composite aerogel, namely the biomass-based composite aerogel. The biomass-based composite aerogel prepared by the method has high porosity, low density and large specific surface area, and has great application potential in the aspect of efficient removal of heavy metal ions and dyes in wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aerogel preparation, and specifically relates to a biomass-based composite aerogel and a preparation method and application thereof. Background Art

[0002] Dyes (such as methyl orange, methylene blue, Congo red, crystal violet, etc.) and heavy metal ions (such as chromium, copper, lead, etc.) discharged from industrial production such as metallurgy, textiles, and mining have caused serious pollution to the water environment. Adsorption is a common water treatment method. Traditional adsorption materials (such as activated carbon and polyacrylamide) have low adsorption capacity, large consumption, and are difficult to regenerate. Metal-organic framework (MOF) is an emerging material with a large specific surface area, adjustable pore size, and diverse chemical composition, showing efficient removal of pollutants. However, most MOF materials in the prior art are powder or granular, which are difficult to recycle and easily cause secondary pollution; the recycling process of some recyclable MOF materials is complicated, and the materials used are expensive. For example, the MOF complex with the structural formula [Zn(L)2(2H2O)]·4H2O provided by patent CN108355611B is in powder form. Although it can be reused, it is difficult to recycle and the cost of use is relatively high. Therefore, researchers have proposed a new idea for material preparation that combines MOF materials with shape-controllable, reusable, and low-cost matrix materials. Biomass aerogel is a three-dimensional porous structure material made from biomass materials that are widely available and low-cost in nature through a sol-gel process and specific drying technology. It has high porosity, large specific surface area, and contains a large number of active functional groups, which helps to achieve stable and uniform loading of MOF materials.

[0003] Cellulose nanofibers (CNF) and chitosan (CS) are common biomass materials in nature. They are low-priced, widely available, and renewable. They also contain abundant active functional groups such as hydroxyl, carboxyl, and amino groups. Using them as the substrate to construct aerogels not only helps to stably and evenly load functional nanomaterials, but also facilitates the efficient adsorption of heavy metal ions and dyes. Montmorillonite (MMT) is a cheap, abundant, and environmentally friendly material with a unique layered structure. It can interact with biomass materials to adjust the pore size of aerogels and enhance their mechanical strength. At the same time, the hydroxyl groups on the surface of montmorillonite further provide more adsorption sites for heavy metal ions and dye molecules.

[0004] There are already some related patents related to aerogel technology in the prior art. For example, patent CN112657437A provides a method for preparing biomass-based composite aerogels, which uses biomass-based waste as raw materials and adopts a "full-component self-assembly method". The preparation process is simple, and the obtained composite aerogel has excellent mechanical properties. However, the material has a single function and is only used for adsorption. The functional material is loaded in a mixed stirring manner, which has poor stability and poor reusability. CN106861626B discloses an adsorption-photocatalytic dual-functional material and its preparation method and application in a volatile organic gas treatment process. The material has high VOCs adsorption capacity selectivity and visible light photocatalytic degradation efficiency, simple process, low energy consumption, and can achieve semi-continuous deep purification of VOCs-containing waste gas. However, the material prepared in this patent is granular, difficult to recycle, and easy to cause secondary pollution. CN116173923B discloses a method for preparing a titanium dioxide-loaded MOFs-based aerogel. The titanium dioxide-loaded MOFs-based aerogel has a large specific surface area, a high porosity, is rich in strongly chelating carboxyl groups, has photocatalytic properties and resistance to biological contamination, and is easily recyclable and reusable. However, the patented material is only used for selective adsorption and reduction of uranyl, and has a narrow application range. Moreover, the TiO2 used in the patent only responds under ultraviolet light, cannot maximize the use of solar energy, and has a low photocatalytic efficiency.

[0005] In summary, the materials used for heavy metal and dye wastewater treatment in the prior art have single functions, poor mechanical properties, low treatment efficiency, and are difficult to reuse. There is a lack of multifunctional biomass-based composite aerogels that can be applied to heavy metal and dye treatment, adsorption and synergistic photocatalytic degradation, and can be recycled and reused. Summary of the invention

[0006] The prior art lacks multifunctional biomass-based composite aerogels that can be applied to heavy metal and dye treatment, adsorption and photocatalytic degradation, and can be recycled and reused. Based on this situation, the present invention provides a biomass-based composite aerogel and its preparation method and application. The biomass-based composite aerogel can be used for the adsorption of heavy metal ions or the adsorption and degradation of dyes in wastewater, which is a more green, efficient and multifunctional way to treat complex wastewater.

[0007] This application proposes a new material preparation idea that combines MOF materials with shape-controllable and reusable matrix materials, and stably loads the heterojunction CdS@UiO-66-NH2 based on MOF materials on the CCM aerogel matrix material by an in-situ generation method. UiO-66-NH2 has a large specific surface area, excellent thermal stability and chemical stability, and can be excited to generate electron-hole pairs under visible light to degrade organic pollutants. However, due to the limitation of rapid recombination of photogenerated carriers, the photocatalytic activity of a single UiO-66-NH2 is low. CdS, as a semiconductor material, is anchored on the surface of UiO-66-NH2 to form a CdS@UiO-66-NH2 photocatalytic heterojunction, which can realize the rapid transfer of photogenerated electron-hole pairs, thereby effectively inhibiting the recombination of photogenerated carriers and improving the photocatalytic degradation efficiency of organic pollutants. In addition, UiO-66-NH2, as a supporting matrix for the stable and uniform loading of CdS nanoparticles, can prevent the aggregation of CdS nanoparticles. Therefore, realizing the synergistic effect of adsorption-photocatalytic degradation on biomass-based aerogels is an effective means for efficient removal of dyes from wastewater and recycling of aerogels.

[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0009] One of the technical solutions of the present invention provides a method for preparing a biomass-based composite aerogel, comprising the following steps:

[0010] (1) Preparation of cellulose nanofiber / chitosan / montmorillonite (CCM) aerogel matrix material:

[0011] S1 dissolving cellulose nanofibers in an acetic acid aqueous solution, stirring and ultrasonicating to disperse and remove bubbles, to obtain a uniform solution;

[0012] S2: adding chitosan, montmorillonite nanosheets and deionized water to the solution obtained in step S1 in sequence, stirring evenly to obtain a mixed solution;

[0013] S3: pouring the mixed solution obtained in step S2 into a mold, and freeze-drying to obtain a cellulose nanofiber / chitosan / montmorillonite (CCM) aerogel matrix material;

[0014] (2) Preparation of UiO-66-NH2 / CCM aerogel:

[0015] S4: soaking the CCM aerogel matrix material obtained in step S3 in a ZrCl4 solution to obtain a mixture;

[0016] S5: adding the 2-amino-1,4-phthalic acid solution to the mixture obtained in step S4, and stirring to obtain a mixed solution;

[0017] S6: adding acetic acid to the mixed solution obtained in step S5, placing the mixed solution in a high pressure reactor, and heating the mixture to obtain a product;

[0018] S7: washing the product obtained in step S6 with N,N-dimethylformamide and methanol in sequence, and then vacuum drying to obtain UiO-66-NH2 / CCM aerogel;

[0019] (3) Preparation of CdS@UiO-66-NH2 / CCM biomass-based composite aerogel materials:

[0020] S8: immersing the UiO-66-NH2 / CCM aerogel obtained in step S7 in a cadmium acetate solution and heating it in a water bath to obtain a mixture;

[0021] S9: adding the sulfide solution to the mixture obtained in step S8, stirring at a constant water bath temperature, taking out and rinsing with deionized water to a neutral pH, and vacuum drying to obtain a CdS@UiO-66-NH2 / CCM composite aerogel material, which is the biomass-based composite aerogel.

[0022] Furthermore, in step S1, the cellulose nanofibers are dissolved in an acetic acid aqueous solution, first stirred for 10 to 30 minutes to be dispersed evenly without lumps, and then ultrasonicated for 10 to 30 minutes to remove bubbles to obtain a uniformly dispersed solution; the concentration of the acetic acid aqueous solution is 1wt% to 5wt%, and the ratio of cellulose nanofibers to the acetic acid aqueous solution is 0.1 to 1.0g:15mL.

[0023] Furthermore, in step S2, chitosan, montmorillonite nanosheets and deionized water are sequentially added to the solution obtained in step S1 under magnetic stirring; the ratio of chitosan, montmorillonite nanosheets, deionized water and the acetic acid aqueous solution in step S1 is 0.1-0.5 g: 0.1-0.5 g: 13-14.7 mL: 15 mL; the addition of deionized water in this step is for dilution, and deionized water cannot be directly added to the acetic acid aqueous solution in S1, because the low concentration of acetic acid used at the beginning cannot completely dissolve the chitosan.

[0024] Furthermore, in step S3, after the mixed solution obtained in step S2 is poured into the mold, it is first placed in a refrigerator at -40 to -10°C for 8 to 24 hours, and then placed in a freeze dryer for freeze drying for 30 to 80 hours to obtain a cellulose nanofiber / chitosan / montmorillonite CCM aerogel matrix material; the mold is preferably a disposable bacterial culture dish with a diameter of 3 to 10 cm.

[0025] Furthermore, in step S4, the ratio of the CCM aerogel matrix material to the ZrCl4 solution is 0.1-0.3 g: 6.0-9.0 mL; the ZrCl4 powder is dissolved in N,N-dimethylformamide and stirred for 10-30 min to obtain the ZrCl4 solution; the concentration of the ZrCl4 solution is 0.02-0.05 g / mL.

[0026] Furthermore, in step S5, the ratio of the volume of the 2-amino-1,4-phthalic acid solution to the CCM aerogel matrix material in step S4 is 6.0-9.0 mL: 0.1-0.3 g; 2-amino-1,4-phthalic acid is dissolved in N,N-dimethylformamide and stirred for 10-30 min to obtain a 2-amino-1,4-phthalic acid solution; the concentration of the 2-amino-1,4-phthalic acid solution is 0.01-0.05 g / mL.

[0027] Furthermore, in step S6, the ratio of the volume of the acetic acid to the CCM aerogel matrix material in step S4 is 2.0-3.0 mL: 0.1-0.3 g; the concentration of the acetic acid is 99.5 wt %; and the mixture is heated in a high pressure reactor at 100-150° C. for 18-30 h.

[0028] Furthermore, in step S7, the vacuum drying temperature is 100-150° C., and the duration is 10-20 hours.

[0029] Furthermore, in step S8, the solvent in the cadmium acetate solution is deionized water with a concentration of 0.001 to 0.0066 g / mL; the water bath is heated to 40 to 80° C. for 0.5 to 1 h.

[0030] Further, in step S9, the sulfide is selected from any one of sodium sulfide nonahydrate, thioacetamide (TAA), and thiourea, preferably sodium sulfide nonahydrate; taking sodium sulfide nonahydrate solution as an example, the solvent in the sodium sulfide nonahydrate solution is deionized water, and the concentration is 0.001-0.01 g / mL; the sodium sulfide nonahydrate solution needs to be added dropwise to the mixture obtained in S8; the temperature of the constant temperature water bath is 40-80°C; the neutral pH is 6.5-7.5; the vacuum drying conditions are 40-100°C for 10-20h.

[0031] The second technical solution of the present invention provides a CdS@UiO-66-NH2 / CCM composite aerogel material prepared by the above technical solution, namely, a biomass-based composite aerogel.

[0032] The third technical solution of the present invention provides an application of CdS@UiO-66-NH2 / CCM biomass-based composite aerogel, which is the adsorption of heavy metal ions in wastewater or the adsorption and degradation of dyes when treating wastewater.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) Using low-cost, environmentally friendly cellulose nanofibers, chitosan, and montmorillonite as raw materials, a three-dimensional porous CCM aerogel matrix material with stable structure and good mechanical properties was constructed, which has the advantages of high porosity, low density, and large specific surface area. The CCM aerogel matrix material can provide an excellent platform for the stable and uniform loading of functional nanomaterials and provide abundant adsorption sites for heavy metal ions and dye molecules.

[0035] (2) The in situ generated CdS@UiO-66-NH2 photocatalytic heterojunction can promote the rapid transfer of photogenerated carriers, inhibit the recombination of photogenerated carriers, effectively improve the photocatalytic efficiency, and achieve complete degradation of the dye.

[0036] (3) By regulating the gradual in situ generation and loading of CdS@UiO-66-NH2 heterojunction, a multifunctional biomass-based composite aerogel was prepared that can achieve efficient adsorption of heavy metal ions and dye molecules and photocatalytic degradation of dye molecules.

[0037] (4) The CdS@UiO-66-NH2 photocatalytic heterojunction was tightly anchored on the surface of biomass-based aerogel through an in situ generation method to achieve stable and uniform loading of nanoparticles. The CdS@UiO-66-NH2 photocatalytic heterojunction was recovered through the desorption of heavy metal ions and the photocatalytic degradation of organic dyes, thereby improving its reusability. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a physical picture of CdS / UiO-66-NH2 / CCM composite aerogel placed on a dandelion flower;

[0039] Figure 2 ATR-FTIR spectra of cellulose nanofiber / chitosan aerogel (CC), cellulose nanofiber / chitosan / montmorillonite aerogel (CCM), UiO-66-NH2 / CCM aerogel, and CdS@UiO-66-NH2 / CCM aerogel;

[0040] Figure 3 is the standard curve of methylene blue concentration and absorbance;

[0041] Figure 4 This is a diagram showing the adsorption and synergistic photocatalytic degradation effect of methylene blue dye on CdS@UiO-66-NH2 / CCM aerogel under simulated visible light. DETAILED DESCRIPTION

[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. The following embodiments are only exemplary illustrations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies realized based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0043] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0044] Example 1

[0045] A method for preparing a multifunctional biomass-based composite aerogel specifically comprises the following steps:

[0046] S1: 0.15 g of cellulose nanofibers were dissolved in 15 mL of 2 wt % acetic acid aqueous solution, stirred for 15 min to disperse evenly without lumps, and ultrasonicated for 15 min to remove bubbles to obtain a cellulose nanofiber solution.

[0047] S2: Weigh 0.15 g chitosan and 0.15 g montmorillonite nanosheets respectively, add them into the cellulose nanofiber solution in sequence under magnetic stirring, and then add 14.55 mL deionized water to obtain a cellulose nanofiber / chitosan / montmorillonite mixed solution.

[0048] S3: pour the mixed solution into a disposable bacterial culture dish with a diameter of 3 cm, put it into a refrigerator at -20°C for 8 h, and put it into a freeze dryer for 36 h to obtain a cellulose nanofiber / chitosan / montmorillonite (CCM) aerogel matrix material.

[0049] S4: 0.233 g ZrCl4 powder was dissolved in 7.0 mL N,N-dimethylformamide and stirred for 15 min to obtain liquid A. The obtained CCM aerogel matrix material was immersed in liquid A.

[0050] S5: 0.166 g of 2-amino-1,4-phthalic acid was dissolved in 7.0 mL of N,N-dimethylformamide and stirred for 15 min to obtain liquid B. Liquid B was slowly added to the mixture obtained in step S4, mixed and stirred for 20 min, and 2.33 mL of 99.5 wt% acetic acid was added.

[0051] S6: Pour the above mixture into a high pressure reactor and heat at 120°C for 18h.

[0052] S7: The product obtained in step S6 is washed three times with N,N-dimethylformamide and methanol respectively, and vacuum dried at 120° C. for 15 h to obtain UiO-66-NH2 / CCM aerogel.

[0053] S8: 0.15 g of cadmium acetate and 0.5 g of sodium sulfide nonahydrate were dissolved in 50 mL of deionized water, respectively, and the obtained composite aerogel was immersed in the cadmium acetate solution and heated to 40° C. in a water bath.

[0054] S9: adding sodium sulfide nonahydrate solution dropwise to the mixture obtained in step S8, stirring at a constant water bath temperature of 40° C., taking out the composite aerogel material, rinsing to a neutral pH, and vacuum drying at 100° C. for 10 h to obtain a CdS@UiO-66-NH2 / CCM composite aerogel material.

[0055] Example 2

[0056] A method for preparing a multifunctional biomass-based composite aerogel specifically comprises the following steps:

[0057] S1: 0.45 g of cellulose nanofibers were dissolved in 15 mL of 3 wt % acetic acid aqueous solution, stirred for 15 min to disperse evenly without lumps, and ultrasonicated for 15 min to remove bubbles to obtain a cellulose nanofiber solution.

[0058] S2: Weigh 0.15 g chitosan and 0.15 g montmorillonite nanosheets respectively, add them into the cellulose nanofiber solution in sequence under magnetic stirring, and then add 14.25 mL deionized water to obtain a cellulose nanofiber / chitosan / montmorillonite mixed solution.

[0059] S3: pour the mixed solution into a disposable bacterial culture dish with a diameter of 3 cm, put it into a refrigerator at -20°C for 8 h, and put it into a freeze dryer for 40 h to obtain a cellulose nanofiber / chitosan / montmorillonite (CCM) aerogel matrix material.

[0060] S4: 0.233 g ZrCl4 powder was dissolved in 7.0 mL N,N-dimethylformamide and stirred for 20 min to obtain liquid A; the obtained CCM aerogel matrix material was immersed in liquid A.

[0061] S5: 0.166 g of 2-amino-1,4-phthalic acid was dissolved in 7.0 mL of N,N-dimethylformamide and stirred for 20 min to obtain liquid B; liquid B was slowly added to the mixture obtained in step S4, mixed and stirred for 20 min, and 2.33 mL of 99.5 wt % acetic acid was added.

[0062] S6: Pour the above mixture into a high pressure reactor and heat at 100°C for 20 h.

[0063] S7: The product obtained in step S6 is washed three times with N,N-dimethylformamide and methanol respectively, and vacuum dried at 100° C. for 20 h to obtain UiO-66-NH2 / CCM aerogel.

[0064] S8: 0.22 g of cadmium acetate and 0.18 g of sodium sulfide nonahydrate were dissolved in 40 mL of deionized water, respectively, and the obtained composite aerogel was immersed in the cadmium acetate solution and heated to 40° C. in a water bath.

[0065] S9: adding sodium sulfide nonahydrate solution dropwise to the mixture obtained in step S8, stirring at a constant water bath temperature of 40° C., taking out the composite aerogel material, rinsing to a neutral pH, and vacuum drying at 100° C. for 10 h to obtain a CdS@UiO-66-NH2 / CCM composite aerogel material.

[0066] Example 3

[0067] A method for preparing a multifunctional biomass-based composite aerogel specifically comprises the following steps:

[0068] S1: 0.45 g of cellulose nanofibers were dissolved in 15 mL of 3 wt % acetic acid aqueous solution, stirred for 20 min to disperse evenly without lumps, and ultrasonicated for 20 min to remove bubbles to obtain a cellulose nanofiber solution.

[0069] S2: Weigh 0.45 g chitosan and 0.15 g montmorillonite nanosheets respectively, add them into the cellulose nanofiber solution in sequence under magnetic stirring, and then add 13.95 mL deionized water to obtain a cellulose nanofiber / chitosan / montmorillonite mixed solution.

[0070] S3: Pour the mixed solution into a disposable bacterial culture dish with a diameter of 3 cm, put it into a refrigerator at -40°C for 10 h, and put it into a freeze dryer for 46 h to obtain a cellulose nanofiber / chitosan / montmorillonite (CCM) aerogel matrix material.

[0071] S4: 0.233 g ZrCl4 powder was dissolved in 7.0 mL N,N-dimethylformamide and stirred for 15 min to obtain liquid A. The obtained CCM aerogel matrix material was immersed in liquid A.

[0072] S5: 0.166 g of 2-amino-1,4-benzenedicarboxylic acid was dissolved in 7.0 mL of N,N-dimethylformamide and stirred for 15 min to obtain liquid B. Liquid B was slowly added to the mixture obtained in step S4, mixed and stirred for 30 min, and 2.33 mL of 99.5 wt% acetic acid was added.

[0073] S6: Pour the above mixture into a high pressure reactor and heat at 120°C for 18h.

[0074] S7: The product obtained in step S6 is washed three times with N,N-dimethylformamide and methanol respectively, and vacuum dried at 120° C. for 15 h to obtain UiO-66-NH2 / CCM aerogel.

[0075] S8: 0.25 g of cadmium acetate and 0.28 g of sodium sulfide nonahydrate were dissolved in 50 mL of deionized water, respectively, and the obtained composite aerogel was immersed in the cadmium acetate solution and heated to 50° C. in a water bath.

[0076] S9: adding sodium sulfide nonahydrate solution dropwise to the mixture obtained in step S8, stirring at a constant water bath temperature of 50° C., taking out the composite aerogel material, rinsing to a neutral pH, and vacuum drying at 80° C. for 14 h to obtain a CdS@UiO-66-NH2 / CCM composite aerogel material.

[0077] Example 4

[0078] A method for preparing a multifunctional biomass-based composite aerogel specifically comprises the following steps:

[0079] S1: 0.75 g of cellulose nanofibers were dissolved in 15 mL of 2 wt % acetic acid aqueous solution, stirred for 20 min to disperse evenly without lumps, and ultrasonicated for 20 min to remove bubbles to obtain a cellulose nanofiber solution.

[0080] S2: Weigh 0.45 g chitosan and 0.15 g montmorillonite nanosheets respectively, add them into the cellulose nanofiber solution in sequence under magnetic stirring, and then add 13.65 mL deionized water to obtain a cellulose nanofiber / chitosan / montmorillonite mixed solution.

[0081] S3: Pour the mixed solution into a disposable bacterial culture dish with a diameter of 3 cm, put it into a refrigerator at -40°C for 10 h, and put it into a freeze dryer for 50 h to obtain a cellulose nanofiber / chitosan / montmorillonite (CCM) aerogel matrix material.

[0082] S4: 0.233 g ZrCl4 powder was dissolved in 7.0 mL N,N-dimethylformamide and stirred for 20 min to obtain liquid A. The obtained CCM aerogel matrix material was immersed in liquid A.

[0083] S5: 0.166 g of 2-amino-1,4-benzenedicarboxylic acid was dissolved in 7.0 mL of N,N-dimethylformamide and stirred for 20 min to obtain liquid B. Liquid B was slowly added to the mixture obtained in step S4, mixed and stirred for 30 min, and 2.33 mL of 99.5 wt% acetic acid was added.

[0084] S6: Pour the above mixture into a high pressure reactor and heat at 120°C for 15h.

[0085] S7: The product obtained in step S6 is washed three times with N,N-dimethylformamide and methanol respectively, and vacuum dried at 100° C. for 20 h to obtain UiO-66-NH2 / CCM aerogel.

[0086] S8: 0.33 g of cadmium acetate and 0.25 g of sodium sulfide nonahydrate were dissolved in 50 mL of deionized water, respectively, and the obtained composite aerogel was immersed in the cadmium acetate solution and heated to 50° C. in a water bath.

[0087] S9: adding sodium sulfide nonahydrate solution dropwise to the mixture obtained in step S8, stirring at a constant water bath temperature of 50° C., taking out the composite aerogel material, rinsing to a neutral pH, and vacuum drying at 80° C. for 12 h to obtain a CdS@UiO-66-NH2 / CCM composite aerogel material.

[0088] Comparative Example 1

[0089] Steps S1 to S7 are the same as those in Example 4 without subsequent steps, and UiO-66-NH2 / CCM aerogel is obtained.

[0090] Comparative Example 2

[0091] Steps S1 to S3 are the same as those in Example 4 without subsequent steps, and CCM aerogel is obtained.

[0092] Comparative Example 3

[0093] S1: 0.75 g of cellulose nanofiber powder was dissolved in 15 mL of 3 wt % acetic acid aqueous solution, stirred for 15 min to disperse evenly without lumps, and ultrasonicated for 15 min to remove bubbles to obtain a cellulose nanofiber solution.

[0094] S2 weighed 0.45 g of chitosan powder, added to the cellulose nanofiber solution under magnetic stirring, and then added 13.8 mL of deionized water to obtain a cellulose nanofiber / chitosan mixed solution.

[0095] S3: Pour the mixed solution into a disposable bacterial culture dish with a diameter of 3 cm, put it into a refrigerator at -40°C for 8 h, and put it into a freeze dryer for 36 h to obtain cellulose nanofiber / chitosan (CC) aerogel.

[0096] Example Effect Measurement

[0097] (I) Characterization and testing of CdS@UiO-66-NH2 / CCM composite aerogel materials

[0098] Figure 1 The CdS@UiO-66-NH2 / CCM composite aerogel prepared in Example 1 has a mass of about 0.4 g and a volume of about 7.09 cm 3 , density is about 0.056g / cm 3 , and can be stably placed on a dandelion flower without bending the petals, indicating the lightweight properties of the resulting composite aerogel.

[0099] The CdS@UiO-66-NH2 / CCM composite aerogel prepared in the above Example 4, the UiO-66-NH2 / CCM aerogel prepared in Comparative Example 1, the CCM aerogel prepared in Comparative Example 2 and the CC aerogel prepared in Comparative Example 3 were characterized. Figure 2 ATR-FTIR spectrum, the spectrum of CC aerogel is located at 3360cm -1 The broad band at 2900 cm corresponds to the overlap of OH and NH stretching vibrations, while the -1 The peak near 1571 cm is attributed to CH stretching bending. -1 The features observed at 1065–1157 cm-1 are derived from the NH bending vibrations of primary and secondary amines. -1 The characteristic peaks in the range of 1418 cm-1 are related to the stretching of CNH / COC and the bending of COH groups. -1 The absorption band at 661cm is due to the shear vibration of -CH2. -1 The peak of is generated by the out-of-plane bending vibration of OH, indicating the successful cross-linking of CS and CNF. The spectrum of CCM aerogel shows a peak at 3690 cm -1 The band at 1030 cm is attributed to the stretching vibration of Si-OH. -1 and 915cm -1 The main peaks at 660 cm-1 correspond to the Si-OH stretching vibration and the O-Si-O stretching vibration, respectively, indicating the successful addition of montmorillonite nanosheets to CNF and CS. The spectra of UiO-66-NH2 / CCM aerogel and CdS@UiO-66-NH2 / CCM aerogel show that the main peak at 660 cm-1 -1 and 766cm -1 The two bands at 1571 cm correspond to the asymmetric stretching of CH and OH. -1 and 1380cm -1 The band at 1492 cm is the signal of asymmetric and symmetric stretching of OCO in the ligand. -1 The weak band at represents the C=C of the benzene ring, proving the successful loading of the CdS@UiO-66-NH2 heterojunction.

[0100] (II) Biomass-based composite aerogel for copper ions (Cu 2+ ) Adsorption performance test

[0101] In this experiment, the CdS@UiO-66-NH2 / CCM aerogel, UiO-66-NH2 / CCM aerogel, CCM aerogel and CC aerogel obtained in Example 4, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were subjected to copper ion (Cu 2+ )Adsorption performance test.

[0102] The test method is as follows: 100 mg of the above four composite aerogel materials are weighed respectively, and they are placed in 30 mL of a copper ion solution with a concentration of 100 mg / L to start adsorption. The copper ion solution after adsorption equilibrium is taken, sodium diethyldithiocarbamate (SDDT) is used as a color developer, and the absorbance is recorded at a wavelength of 447 nm using a UV-Vis spectrophotometer. The concentration of copper ions is calculated based on the absorbance, and then the adsorption rate of copper ions by the four aerogels is calculated according to the following formula. The results are shown in Table 1.

[0103] The calculation formula of adsorption rate is:

[0104]

[0105] C0 is the initial concentration of methylene blue, and Ce is the adsorption equilibrium concentration.

[0106] Table 1 Copper ion adsorption results of Example 4 and Comparative Examples 1 to 3

[0107]

[0108] The above results show that pure CC aerogel has the lowest adsorption rate for copper ions, which is 60%; the adsorption rate of CCM aerogel for copper ions is 65%, which indicates that the hydroxyl groups on the surface of montmorillonite provide more adsorption sites for copper ions; after loading the MOF material UiO-66-NH2, the adsorption rate of UiO-66-NH2 / CCM aerogel for copper ions is the highest, which is 78%, proving that the loading of UiO-66-NH2 provides a large number of adsorption sites for the aerogel material; and after adding CdS nanoparticles, the adsorption rate of CdS@UiO-66-NH2 / CCM aerogel is slightly lower than that of UiO-66-NH2 / CCM aerogel, which is attributed to the fact that CdS nanoparticles occupy a small number of adsorption sites during the loading process, resulting in a decrease in the adsorption rate of copper ions by the sample.

[0109] (III) Synergistic test of dye adsorption and photocatalytic degradation by biomass-based composite aerogels

[0110] The CdS@UiO-66-NH2 / CCM aerogel, UiO-66-NH2 / CCM aerogel, CCM aerogel and CC aerogel obtained in Example 4, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested for the adsorption synergistic photocatalytic degradation of methylene blue dye.

[0111] The test method is as follows: 100 mg of the above four composite aerogel materials are weighed respectively, and they are placed in 30 mL of a 50 mg / L methylene blue solution. After reaching adsorption equilibrium, they are degraded under simulated visible light. The methylene blue solution after 6 hours of illumination is taken, and the absorbance is recorded at a wavelength of 664 nm using a UV-Vis spectrophotometer. The absorbance is proportional to the content of methylene blue, which can be calculated according to the formula A = 0.1796C + 0.039 (R 2 =0.9957, where A represents absorbance, C represents concentration, and the standard curve is shown in Figure 1. Figure 3 ) was used to calculate the concentration of methylene blue dye, and then the removal rates of methylene blue dye by the four aerogels were calculated according to the following formula. The results are shown in Table 2.

[0112] The calculation formula for the removal rate is:

[0113]

[0114] C0 is the initial concentration of methylene blue, C t is the concentration of methylene blue at time t.

[0115] Table 2 Results of the synergistic photocatalytic degradation of methylene blue dye adsorption in Example 4 and Comparative Examples 1 to 3

[0116]

[0117] The above results show that the removal rates of pure CC aerogel and CCM aerogel with montmorillonite for methylene blue dye are 78.9% and 83.7%, respectively. This is because the addition of montmorillonite provides more adsorption sites for methylene blue dye. The removal rate of UiO-66-NH2 / CCM aerogel for methylene blue dye reaches 91.1%. This is because the MOF material UiO-66-NH2 can be excited to generate electron-hole pairs under visible light to degrade methylene blue dye while providing more adsorption sites. However, due to the limitation of rapid recombination of photogenerated carriers, the photocatalytic activity of single UiO-66-NH2 is low. The removal rate of CdS@UiO-66-NH2 / CCM aerogel for methylene blue dye is as high as 99.5%, which is attributed to the fact that the CdS@UiO-66-NH2 photocatalytic heterojunction can effectively inhibit the recombination of photogenerated carriers and improve the photocatalytic degradation efficiency.

[0118] in addition, Figure 4The UV-visible spectrum scanning results of the CdS@UiO-66-NH2 / CCM composite aerogel prepared in Example 4 in the adsorption synergistic photocatalytic degradation test of methylene blue are provided. The black curve is the spectrum scanning result of the methylene blue dye before treatment, and the red curve is the spectrum scanning result of the methylene blue dye after the composite aerogel adsorption synergistic photocatalytic degradation. Comparing the absorbance of the two groups of curves at 664nm, it is shown that the CdS@UiO-66-NH2 / CCM composite aerogel has a good adsorption synergistic photocatalytic degradation effect on methylene blue dye.

[0119] (IV) Recyclability of biomass-based composite aerogels

[0120] The CdS@UiO-66-NH2 / CCM composite aerogel prepared in Example 4 was subjected to 5 adsorption / desorption and photocatalytic degradation cycle tests.

[0121] The test method is as follows: 100 mg of the composite aerogel material is put into 30 mL of a copper ion solution with a concentration of 100 mg / L, and the copper ion solution after reaching adsorption equilibrium is taken, and sodium diethyldithiocarbamate (SDDT) is used as a color developer, and the absorbance is recorded at a wavelength of 447 nm using a UV-Vis spectrophotometer. Then, a 0.1 M HNO3 solution is used as a desorbent, and the composite aerogel adsorbent is stirred for 480 min under 0.1 M HNO3, thoroughly rinsed with deionized water, and then vacuum dried at 60 ° C for 12 h for the next round of adsorption-desorption. Adsorption and desorption are repeated 5 times to test the reusability of the composite aerogel adsorbed copper ions, and the results are shown in Table 3. 100 mg CdS@UiO-66-NH2 / CCM composite aerogel sample was put into 30 mL of 50 mg / L methylene blue solution and degraded under simulated visible light. The methylene blue solution was taken after 6 hours of illumination, and the absorbance was recorded at 664 nm using a UV-Vis spectrophotometer. The aerogel sample was then taken out, washed with deionized water several times, and vacuum dried at 60 ° C for 12 hours for the next round of photocatalytic degradation. The cycle was repeated 5 times to test the reusability of the composite aerogel photocatalytic degradation of methylene blue solution. The results are shown in Table 3.

[0122] Table 3 Adsorption / desorption and photocatalytic degradation cycle test results of Example 4

[0123]

[0124] The above results show that the adsorption performance and photocatalytic degradation performance decrease slightly with the increase of the number of cycles. After 5 cycles, the adsorption rate of copper ions by CdS@UiO-66-NH2 / CCM composite aerogel is 68%, and the removal rate of methylene blue is 93%, with good recycling performance. The decrease in the adsorption rate of copper ions by the aerogel is due to the loss of active sites in the aerogel during the cycle, while the decrease in the removal rate of methylene blue is attributed to the loss of CdS@UiO-66-NH2 photocatalytic heterojunction during the cycle.

[0125] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a biomass-based composite aerogel, characterized in that: The following steps are involved: (1) Preparation of CCM aerogel matrix material: Using cellulose nanofibers, chitosan, and montmorillonite nanosheets as raw materials, acetic acid aqueous solution as solvent, and deionized water as diluent, a CCM aerogel matrix material was prepared; (2) Preparation of UiO-66-NH2 / CCM aerogel: CCM aerogel matrix material was immersed in ZrCl4 solution, stirred evenly and then added with 2-amino-1,4-phthalic acid solution to obtain a mixture; acetic acid was added to the mixture and placed in a high pressure reactor, heated, washed and vacuum dried to obtain UiO-66-NH2 / CCM aerogel; (3) Preparation of CdS@UiO-66-NH2 / CCM composite aerogel material: The UiO-66-NH2 / CCM aerogel prepared in step (2) is immersed in a cadmium acetate solution and heated in a water bath to obtain a mixture; a sulfide solution is added to the mixture, and after stirring under constant temperature, the mixture is taken out, rinsed, and vacuum dried to obtain a CdS@UiO-66-NH2 / CCM composite aerogel material, which is the biomass-based composite aerogel.

2. The method for preparing a biomass-based composite aerogel according to claim 1, characterized in that: In step (1), cellulose nanofibers are first dissolved in an acetic acid aqueous solution, stirred for 10 to 30 minutes to be dispersed evenly without lumps, and then ultrasonicated for 10 to 30 minutes to remove bubbles; chitosan, montmorillonite nanosheets, and deionized water are then added in sequence under magnetic stirring to obtain a uniform mixed solution; finally, the mixed solution is frozen at -40 to -10°C for 8 to 24 hours and then placed in a freeze dryer for 30 to 80 hours for freeze drying to obtain a CCM aerogel matrix material.

3. The method for preparing a biomass-based composite aerogel according to claim 1, characterized in that: In step (1), the addition ratio of the cellulose nanofibers, chitosan, montmorillonite nanosheets, deionized water and acetic acid aqueous solution is 0.1-1.0 g: 0.1-0.5 g: 0.1-0.5 g: 13-14.7 mL: 15 mL; the concentration of the acetic acid aqueous solution is 1 wt% to 5 wt%.

4. The method for preparing a biomass-based composite aerogel according to claim 1, characterized in that: In step (2), the ratio of the CCM aerogel matrix material, ZrCl4 solution, 2-amino-1,4-phthalic acid solution and acetic acid is 0.1-0.3 g: 6.0-9.0 mL: 6.0-9.0 mL: 2.0-3.0 mL; the concentration of the ZrCl4 solution is 0.02-0.05 g / mL; the concentration of the 2-amino-1,4-phthalic acid solution is 0.01-0.05 g / mL; the solvents of the ZrCl4 solution and 2-amino-1,4-phthalic acid are both N,N-dimethylformamide; and the concentration of the acetic acid is 99.5 wt%.

5. The method for preparing a biomass-based composite aerogel according to claim 1, characterized in that: In step (2), the heating temperature in the high-pressure reactor is 100 to 150° C. for 18 to 30 hours; the product obtained after heating is washed with N,N-dimethylformamide and methanol.

6. The method for preparing a biomass-based composite aerogel according to claim 1, characterized in that: In step (2), the vacuum drying is carried out at a temperature of 100 to 150° C. and for a time of 10 to 20 hours.

7. The method for preparing a biomass-based composite aerogel according to claim 1, characterized in that: In step (3), the sulfide is any one of sodium sulfide nonahydrate, thioacetamide, and thiourea; the ratio of the UiO-66-NH2 / CCM aerogel, the cadmium acetate solution and the sulfide solution is 0.1-0.4 g:30-80 mL:30-80 mL; the concentration of the cadmium acetate solution is 0.001-0.0066 g / mL, and it is dissolved in deionized water; when the sulfide solution is a sodium sulfide nonahydrate solution, the concentration is 0.001-0.01 g / mL, and it is dissolved in deionized water.

8. The method for preparing a biomass-based composite aerogel according to claim 1, characterized in that: In step (3), the constant temperature condition is water bath insulation at a temperature of 40 to 80° C. for 0.5 to 1 h; the rinsing operation is rinsing with deionized water until the pH is 6.5-7.5; the vacuum drying temperature is 40 to 100° C. for 10 to 20 h.

9. A biomass-based composite aerogel, characterized in that: It is obtained according to the preparation method according to any one of claims 1 to 8, namely the CdS@UiO-66-NH2 / CCM composite aerogel material.

10. The use of a biomass-based composite aerogel according to claim 9, characterized in that: The biomass-based composite aerogel is used to treat wastewater and adsorb heavy metal ions in the wastewater or adsorb and degrade dyes.

Citation Information

Patent Citations

  • An adsorption-photocatalytic bifunctional material, its preparation method, and its application in volatile organic gas treatment processes.

    CN106861626B

  • A MOF complex, its synthesis, and its application in adsorbing organic dyes in wastewater.

    CN108355611B

  • Biomass-based composite aerogel and preparation method thereof

    CN112657437A

  • A method for preparing MOFs-based aerogel loaded with titanium dioxide

    CN116173923B