Heavy metal capturing agent and preparation method thereof

Through the synergistic effect of modified montmorillonite and dodecyl trimethylammonium bromide, an efficient heavy metal capture agent was prepared, which solved the problems of low efficiency and high cost of heavy metal pollution treatment in the prior art, and realized the wastewater Efficient removal of heavy metal ions.

CN119056400APending Publication Date: 2024-12-03XINJIANG WATER TREATMENT ENG TECH RES CENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411410218.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When dealing with heavy metal pollution in water bodies, the prior art has low treatment efficiency, high cost and is prone to secondary pollution, making it difficult to effectively remove heavy metal ions in wastewater.

Method used

Heavy metal capture agent prepared from raw materials such as montmorillonite, sulfuric acid, dodecyl trimethyl ammonium bromide, diethylene triamine, carbon disulfide, sodium sulfide, carbamate disulfide and sodium hydroxide, and is modified by sulfuric acid. Montmorillonite and combined with dodecyl trimethylammonium bromide increase its specific surface area and porosity to form an efficient precipitate to remove heavy metal ions.

Benefits of technology

The efficient removal of heavy metal ions in wastewater is achieved, the preparation method is simple and low-cost, the generated precipitates are stable, and are not easily degraded or desorbed, which significantly improves the removal efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a heavy metal trapping agent and a preparation method of the heavy metal trapping agent. The sewage treatment agent is mainly prepared from the following raw materials: 10 to 15 parts of montmorillonite, 15 to 25 parts of sulfuric acid, 15 to 25 parts of dodecyl trimethyl ammonium bromide, 10 to 15 parts of diethylenetriamine, 5 to 8 parts of carbon disulfide, 10 to 15 parts of sodium sulfide, 10 to 15 parts of disulfide carbamate, 3 to 8 parts of sodium hydroxide and 15 to 20 parts of deionized water. The heavy metal trapping agent provided by the invention can quickly react with heavy metal ions in wastewater to generate water-insoluble precipitates, so that the heavy metal ions in the wastewater can be efficiently removed, and the heavy metal trapping agent has the characteristics of simple preparation method, low cost and high removal efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of environmental protection technology, and in particular to a heavy metal scavenger and a preparation method thereof. Background Art

[0002] With the acceleration of industrialization, the problem of heavy metal pollution in water bodies is becoming increasingly serious, posing a serious threat to the ecological environment and human health. Water is the material basis for human survival and development, so the problem of water pollution has attracted great attention. Heavy metal ions are one of the main pollutants in the water environment and are potentially harmful. Heavy metal ions such as Hg, Cd, Cr, and As can produce significant toxicity in trace amounts. Not only can they not be degraded by microorganisms, but once they are ingested by organisms, they can be enriched at the upper end of the food chain, which can make proteins, enzymes, etc. lose their activity and cause cumulative poisoning. Therefore, the pollution of heavy metal substances has become a major problem restricting my country's economic and social development and the improvement of people's livelihood. Traditional heavy metal treatment methods such as chemical precipitation, adsorption, and ion exchange have problems such as low treatment efficiency, high cost, and easy secondary pollution. Therefore, it is of great significance to develop an efficient, environmentally friendly, and economical heavy metal capture agent.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The first purpose of the present invention is to provide a heavy metal capture agent, which can react rapidly with heavy metal ions in wastewater to generate water-insoluble precipitates, thereby being able to efficiently remove heavy metal ions in wastewater. The capture agent has the characteristics of simple preparation method, low cost and high removal efficiency.

[0005] The second object of the present invention is to provide a method for preparing a heavy metal scavenger, which has simple operation, low cost and mild operating conditions.

[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: The invention provides a heavy metal scavenger, which is mainly prepared from the following raw materials, by weight: 10-15 parts of montmorillonite, 15-25 parts of sulfuric acid, 15-25 parts of dodecyltrimethylammonium bromide, 10-15 parts of diethylenetriamine, 5-8 parts of carbon disulfide, 10-15 parts of sodium sulfide, 10-15 parts of disulfide carbamate, 3-8 parts of sodium hydroxide and 15-20 parts of deionized water.

[0007] Preferably, as a further specific embodiment, 11-14 parts of montmorillonite, 18-23 parts of sulfuric acid, 17-22 parts of dodecyltrimethylammonium bromide, 11-14 parts of diethylenetriamine, 6-7 parts of carbon disulfide, 11-14 parts of sodium sulfide, 11-14 parts of disulfide carbamate, 5-7 parts of sodium hydroxide and 16-18 parts of deionized water.

[0008] Preferably, as a further specific embodiment, 12 parts of montmorillonite, 20 parts of sulfuric acid, 18 parts of dodecyltrimethylammonium bromide, 12 parts of diethylenetriamine, 6 parts of carbon disulfide, 13 parts of sodium sulfide, 12 parts of disulfide carbamate, 6 parts of sodium hydroxide and 17 parts of deionized water.

[0009] The present invention mainly provides a heavy metal capture agent, which can react rapidly with heavy metal ions in wastewater to generate water-insoluble precipitates, so as to achieve efficient removal of heavy metal ions in wastewater. The selection and dosage of raw materials are very important for the present invention. When the raw materials are 10-15 parts of montmorillonite, 15-25 parts of sulfuric acid, 15-25 parts of dodecyltrimethylammonium bromide, 10-15 parts of diethylenetriamine, 5-8 parts of carbon disulfide, 10-15 parts of sodium sulfide, 10-15 parts of disulfide carbamate, 3-8 parts of sodium hydroxide and 15-20 parts of deionized water, more preferably 12 parts of montmorillonite, 20 parts of sulfuric acid, 18 parts of dodecyltrimethylammonium bromide, 12 parts of diethylenetriamine, 6 parts of carbon disulfide, 13 parts of sodium sulfide, 12 parts of disulfide carbamate, 6 parts of sodium hydroxide and 17 parts of deionized water, the heavy metal capture agent prepared has the best effect. The invention mainly adopts montmorillonite as the main raw material of the metal capture agent. The invention discloses a hydrous silicate mineral having a large specific surface area and a high porosity, which makes montmorillonite have a strong adsorption capacity for heavy metal ions in wastewater. In order to further improve the adsorption effect of montmorillonite on heavy metal ions in wastewater, the present invention modifies montmorillonite by using sulfuric acid and combines it with dodecyltrimethylammonium bromide to further improve the capture effect of montmorillonite on heavy metal ions in wastewater. The addition of sulfuric acid can cause a certain change in the structure of montmorillonite. When montmorillonite is treated with sulfuric acid, the modification of montmorillonite is achieved by sulfuric acid. The montmorillonite is modified by acidification, so that the specific surface area of ​​montmorillonite is increased, and the pore size is also increased, thereby increasing the porosity and specific surface area of ​​montmorillonite, making it have stronger adsorption and chemical activity, improving its adsorption capacity and catalytic performance, so that the prepared heavy metal capture agent can better realize the precipitation of heavy metal ions in wastewater.

[0010] Therefore, it can be known that the amount of sulfuric acid used in the present invention is very important for the present invention. This is because when sulfuric acid is used to modify montmorillonite, as the amount of sulfuric acid increases, the alumina octahedral structure of montmorillonite is gradually destroyed and the layered structure also changes, resulting in a decrease in the cation exchange capacity and sulfuric acid treatment causing the metal oxides in the montmorillonite to dissolve. In particular, when the amount of sulfuric acid used is high, the crystal structure of montmorillonite may collapse, affecting its adsorption effect on heavy metal ions, so that when the interlayer cations are exchanged with the heavy metal ions, the heavy metal ions cannot be fixed in the structure of the montmorillonite, making the precipitate formed by the montmorillonite and the heavy metal ions unstable.

[0011] After montmorillonite is modified by sulfuric acid, dodecyltrimethylammonium bromide is subsequently added to activate the modified montmorillonite. Dodecyltrimethylammonium bromide, as a quaternary ammonium salt surfactant, can be well inserted into the interlayer of montmorillonite, thereby changing the interlayer spacing of the modified montmorillonite, so that the interlayer spacing of the modified montmorillonite is increased and the organic carbon content is increased. Therefore, the present invention realizes the modification and activation of montmorillonite through the synergistic effect of sulfuric acid and dodecyltrimethylammonium bromide, and further improves its adsorption performance for heavy metal ions.

[0012] Finally, by adding diethylenetriamine, carbon disulfide, sodium sulfide, dithiocarbamate and sodium hydroxide, the montmorillonite is further modified, and the heavy metal ions in the wastewater can be adsorbed by the adsorption capacity of the added raw materials themselves, so that the heavy metal ions in the wastewater can be removed efficiently. The modification of montmorillonite by diethylenetriamine can effectively improve the structure of montmorillonite, so that it has better adsorption performance, can effectively adsorb toxic heavy metal ions in water with higher adsorption efficiency, and the formed precipitate is more stable and not easy to be degraded and desorbed; the addition of carbon disulfide can form chelate precipitation with the heavy metal ions in the wastewater. At a suitable pH value, the modified montmorillonite and carbon disulfide and other substances are mutually compatible, so as to achieve efficient removal of heavy metal ions in the wastewater.

[0013] The present invention also provides a method for preparing a heavy metal capture agent, comprising the following steps: After adding montmorillonite and sulfuric acid in sequence, heating to a constant temperature, and then adding deionized water for washing; After the cleaning is completed, dodecyl trimethyl ammonium bromide is added thereto for activation to obtain an activated montmorillonite suspension; Add diethylenetriamine, carbon disulfide, sodium sulfide, dithiocarbamate and sodium hydroxide to the activated montmorillonite suspension, continue the reaction, centrifuge and dry to obtain the product.

[0014] In the preparation process of the heavy metal scavenger of the present invention, sulfuric acid and montmorillonite are first added for modification. The acid treatment can dissolve the interlayer metal cations of the montmorillonite, thereby replacing them with smaller and lower valence hydrogen ions, thereby reducing the van der Waals force between the montmorillonite layers, increasing the interlayer spacing, and also being able to effectively remove impurities in the montmorillonite channels, thereby expanding the specific surface area of ​​the montmorillonite, enhancing the adsorption activity of the modified montmorillonite, and having better adsorption performance.

[0015] Preferably, as a further specific implementation, after montmorillonite and sulfuric acid are added in sequence, the mixture is heated to 90° C.-100° C. and kept at a constant temperature for 3 h-5 h.

[0016] Among them, for the present invention, the temperature of heating after adding montmorillonite and sulfuric acid is very important, because in the process of sulfuric acid modification of montmorillonite, temperature is crucial. When the temperature is 90°C-100°C provided by the present invention, preferably 95°C, the modification effect of sulfuric acid on montmorillonite is optimal. This is because as the temperature increases, the reaction efficiency of sulfuric acid and montmorillonite will be accelerated, and the reaction efficiency is closely related to the modification effect of montmorillonite. When the temperature is too high, the structure of montmorillonite will change. Under high temperature conditions, the layered structure of montmorillonite will be destroyed, resulting in a decrease in its cation exchange capacity, blue absorption capacity and other properties, thereby affecting its adsorption effect on heavy metal ions. In addition, as the temperature increases, the reaction rate of sulfuric acid and montmorillonite will be accelerated, making the modification process faster, which may lead to incomplete modification and affect the adsorption effect of montmorillonite. Therefore, only when the temperature is raised to a suitable range when sulfuric acid is added to modify montmorillonite, the reaction rate of sulfuric acid and montmorillonite can be controlled within a reasonable range, so that the modification effect on montmorillonite is the best.

[0017] Preferably, as a further specific implementation, the cleaning process is to add deionized water to wash the precipitate, rinse to pH=3, and centrifuge for dehydration.

[0018] Preferably, as a further specific implementation manner, the activation time is 1 h-3 h.

[0019] Preferably, as a further specific embodiment, the activation time is 2 hours.

[0020] Preferably, as a further specific implementation manner, the continuous reaction time is 3h-6h.

[0021] Preferably, as a further specific embodiment, the continuous reaction time is 4 hours.

[0022] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention provides a heavy metal scavenger, which can react rapidly with heavy metal ions in wastewater to generate water-insoluble precipitates, thereby being able to efficiently remove heavy metal ions in wastewater. The scavenger has the characteristics of simple preparation method, low cost and high removal efficiency.

[0023] (2) The second object of the present invention is to provide a method for preparing a heavy metal scavenger, which has simple operation, low cost and mild operating conditions. DETAILED DESCRIPTION

[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with specific implementation methods, but those skilled in the art will understand that the embodiments described below are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] In order to more clearly explain the technical solution of the present invention, it is described in the form of specific embodiments below.

[0026] Example 1 The preparation process of the heavy metal capture agent is as follows: Take 10g of montmorillonite, 15g of sulfuric acid, 15g of dodecyltrimethylammonium bromide, 10g of diethylenetriamine, 5g of carbon disulfide, 10g of sodium sulfide, 10g of disulfide carbamate, 3g of sodium hydroxide and 15g of deionized water; 10 g of montmorillonite and 15 g of sulfuric acid were added to the reactor in sequence. The reactor was opened and heated to 90°C and kept at this temperature for 3 hours. Deionized water was added to the reactor to wash the precipitate, and the pH of the rinse was 3, followed by centrifugal dehydration. After centrifugal dehydration, dodecyltrimethylammonium bromide was added thereto for activation for 1 hour to obtain an activated montmorillonite suspension; Then, diethylenetriamine, carbon disulfide, sodium sulfide, dithiocarbamate and sodium hydroxide are added to the activated montmorillonite suspension, and the reaction is continued for 3 hours, followed by centrifugation. After the centrifugation is completed, the suspension is dried to obtain the product.

[0027] Example 2 The preparation process of the heavy metal capture agent is as follows: Take 15g of montmorillonite, 25g of sulfuric acid, 25g of dodecyltrimethylammonium bromide, 15g of diethylenetriamine, 8g of carbon disulfide, 15g of sodium sulfide, 15g of disulfide carbamate, 8g of sodium hydroxide and 20g of deionized water; 15 g of montmorillonite and 25 g of sulfuric acid were added to the reactor in sequence. The reactor was opened and heated to 100°C and kept at this temperature for 5 hours. Deionized water was added to the reactor to wash the precipitate, and the pH of the rinse was 3, followed by centrifugal dehydration. After centrifugal dehydration, 25 g of dodecyltrimethylammonium bromide was added thereto for activation for 3 h to obtain an activated montmorillonite suspension; Then, 15 g of diethylenetriamine, 8 g of carbon disulfide, 15 g of sodium sulfide, 15 g of dithiocarbamate and 8 g of sodium hydroxide were added to the activated montmorillonite suspension, and the reaction was continued for 6 hours, followed by centrifugation. After the centrifugation was completed, the suspension was dried to obtain the product.

[0028] Example 3 The preparation process of the heavy metal capture agent is as follows: Take 12g of montmorillonite, 20g of sulfuric acid, 18g of dodecyltrimethylammonium bromide, 12g of diethylenetriamine, 6g of carbon disulfide, 13g of sodium sulfide, 12g of disulfide carbamate, 6g of sodium hydroxide and 17g of deionized water; 12 g of montmorillonite and 20 g of sulfuric acid were added to the reactor in sequence. The reactor was opened and heated to 95°C and kept at this temperature for 4 hours. Deionized water was added to the reactor to wash the precipitate, and the pH of the rinse was 3, followed by centrifugal dehydration. After centrifugal dehydration, 18 g of dodecyltrimethylammonium bromide was added thereto for activation for 3 h to obtain an activated montmorillonite suspension; Then, 12 g of diethylenetriamine, 6 g of carbon disulfide, 13 g of sodium sulfide, 12 g of dithiocarbamate and 6 g of sodium hydroxide were added to the activated montmorillonite suspension, and the reaction was continued for 5 hours, followed by centrifugation. After the centrifugation was completed, the suspension was dried to obtain the product.

[0029] Example 4 The specific preparation steps of the heavy metal scavenger are consistent with those in Example 3, except that the formula is adjusted to 5g montmorillonite, 10g sulfuric acid, 12g dodecyltrimethylammonium bromide, 8g diethylenetriamine, 4g carbon disulfide, 8g sodium sulfide, 8g dithiocarbamate, 1g sodium hydroxide, and 10g deionized water.

[0030] Example 5 The specific preparation steps of the heavy metal scavenger are consistent with those in Example 3, except that the formula is adjusted to 20g montmorillonite, 26g sulfuric acid, 30g dodecyltrimethylammonium bromide, 20g diethylenetriamine, 10g carbon disulfide, 20g sodium sulfide, 20g dithiocarbamate, 10g sodium hydroxide, and 30g deionized water.

[0031] Example 6 The specific preparation steps of the heavy metal capture agent are the same as those in Example 3, except that the temperature is raised to 150° C. when montmorillonite and sulfuric acid are added to the reactor.

[0032] Example 7 The specific preparation steps of the heavy metal capture agent are the same as those in Example 3, except that the temperature is raised to 80° C. when montmorillonite and sulfuric acid are added to the reactor.

[0033] Example 8 The specific preparation steps of the heavy metal scavenger are the same as those in Example 3, except that when montmorillonite and sulfuric acid are added to the reactor, the constant temperature time after heating is adjusted to 7 hours.

[0034] Example 9 The specific preparation steps of the heavy metal scavenger are the same as those in Example 3, except that when montmorillonite and sulfuric acid are added to the reactor, the constant temperature time after heating is adjusted to 2 hours.

[0035] Example 10 The specific preparation steps of the heavy metal scavenger are the same as those in Example 3, except that the pH is adjusted to 5 when the montmorillonite and sulfuric acid are subjected to constant temperature treatment and then rinsed with deionized water.

[0036] Embodiment 11 The specific preparation steps of the heavy metal capture agent are the same as those in Example 3, except that the activation time is changed to 7 h.

[0037] Comparative Example 1 The specific preparation steps of the heavy metal capture agent are the same as those in Example 3, except that sulfuric acid is replaced by phosphoric acid.

[0038] Comparative Example 2 The specific preparation steps of the heavy metal scavenger are the same as those in Example 3, except that dodecyltrimethylammonium bromide is replaced by lecithin.

[0039] Comparative Example 3 The specific preparation steps of the heavy metal scavenger are the same as those in Example 3, except that the montmorillonite suspension is directly obtained without activation after centrifugal dehydration.

[0040] Comparative Example 4 The specific preparation steps of the heavy metal capture agent are the same as those in Example 3, except that sulfuric acid is replaced by tannic acid.

[0041] Experimental Example 1 Heavy metal removal effect test of heavy metal capture agent: Some electroplating wastewater from an electroplating company was taken and divided into 16 portions, and 500 ppm of the heavy metal scavenger prepared in Examples 1-12 and Comparative Examples 1-4 were added respectively. After stirring for 30 minutes, the heavy metal indicators in the water before and after the reaction were tested respectively. The results are shown in Table 1. Table 1 Experimental results

[0042] It can be seen from Table 1 above that by comparing Examples 1-5 and Comparative Examples 1-4, it can be seen that the amount of each raw material is very important for the present invention. When the raw materials are 10-15 parts of montmorillonite, 15-25 parts of sulfuric acid, 15-25 parts of dodecyltrimethylammonium bromide, 10-15 parts of diethylenetriamine, 5-8 parts of carbon disulfide, 10-15 parts of sodium sulfide, 10-15 parts of disulfide carbamate, 3-8 parts of sodium hydroxide and 15-20 parts of deionized water, more preferably 12 parts of montmorillonite, 20 parts of sulfuric acid, 18 parts of dodecyltrimethylammonium bromide, 12 parts of diethylenetriamine, 6 parts of carbon disulfide, 13 parts of sodium sulfide, 12 parts of disulfide carbamate, 6 parts of sodium hydroxide and 17 parts of deionized water, the prepared heavy metal capture agent has the best effect. It is mainly through the selection of montmorillonite as the main component of the metal capture agent, because it has expansibility and layered structure of hydrous silicate Salt mineral, and due to its large specific surface area and high porosity, montmorillonite has a strong adsorption capacity for heavy metal ions in wastewater. In order to further improve the adsorption effect of montmorillonite on heavy metal ions in wastewater, the present invention modifies montmorillonite by using sulfuric acid, and combines it with dodecyltrimethylammonium bromide, so as to further improve the capture effect of montmorillonite on heavy metal ions in wastewater. The addition of sulfuric acid can cause a certain change in the structure of montmorillonite. When montmorillonite is treated with sulfuric acid, the modification of montmorillonite is achieved by sulfuric acid, and the montmorillonite is modified by acidification, so that the specific surface area of ​​montmorillonite is increased, and the pore size is also increased, thereby increasing the porosity and specific surface area of ​​montmorillonite, making it have stronger adsorption and chemical activity, improving its adsorption capacity and catalytic performance, so that the prepared heavy metal capture agent can better realize the precipitation of heavy metal ions in wastewater.

[0043] By comparing Examples 6-7, it can be known that when montmorillonite is modified by adding sulfuric acid, the heating temperature is very important for the present invention. This is because in the process of sulfuric acid modification of montmorillonite, temperature is crucial. When the temperature is 90°C-100°C provided by the present invention, preferably 95°C, the modification effect of sulfuric acid on montmorillonite is optimal. This is because as the temperature increases, the reaction efficiency of sulfuric acid and montmorillonite will be accelerated, wherein the reaction efficiency is closely related to the modification effect of montmorillonite. When the temperature is too high, the structure of montmorillonite will change. Under high temperature conditions, the layered structure of montmorillonite will be destroyed, resulting in a decrease in its cation exchange capacity, blue absorption capacity and other properties, thereby affecting its adsorption effect on heavy metal ions. In addition, as the temperature increases, the reaction rate of sulfuric acid and montmorillonite will be accelerated, making the modification process faster, which may lead to incomplete modification and affect the adsorption effect of montmorillonite. Therefore, only when the temperature is raised to a suitable range when sulfuric acid is added to modify montmorillonite, the reaction rate of sulfuric acid and montmorillonite can be controlled within a reasonable range, so that the modification effect on montmorillonite is the best.

[0044] By comparing Examples 8-9, it can be seen that when sulfuric acid is used to modify montmorillonite, the constant temperature time is very important for the present invention. This is because sulfuric acid and montmorillonite will react violently when they are in a suitable temperature range. In order to make the modification of montmorillonite by sulfuric acid more complete, the reaction environment of the two is kept at a suitable reaction temperature by means of a constant temperature, so that the reaction rate of sulfuric acid and montmorillonite is controlled within a reasonable range, thereby achieving the best modification effect on montmorillonite.

[0045] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A heavy metal scavenger, characterized in that: The invention is mainly prepared from the following raw materials, by weight: 10-15 parts of montmorillonite, 15-25 parts of sulfuric acid, 15-25 parts of dodecyltrimethylammonium bromide, 10-15 parts of diethylenetriamine, 5-8 parts of carbon disulfide, 10-15 parts of sodium sulfide, 10-15 parts of disulfide carbamate, 3-8 parts of sodium hydroxide and 15-20 parts of deionized water.

2. The heavy metal scavenger according to claim 1, characterized in that 11-14 parts of montmorillonite, 18-23 parts of sulfuric acid, 17-22 parts of dodecyltrimethylammonium bromide, 11-14 parts of diethylenetriamine, 6-7 parts of carbon disulfide, 11-14 parts of sodium sulfide, 11-14 parts of disulfide carbamate, 5-7 parts of sodium hydroxide and 16-18 parts of deionized water.

3. The heavy metal scavenger according to claim 1, characterized in that 12 parts of montmorillonite, 20 parts of sulfuric acid, 18 parts of dodecyltrimethylammonium bromide, 12 parts of diethylenetriamine, 6 parts of carbon disulfide, 13 parts of sodium sulfide, 12 parts of disulfide carbamate, 6 parts of sodium hydroxide and 17 parts of deionized water.

4. A method for preparing a heavy metal scavenger according to any one of claims 1 to 3, characterized in that: The following steps are involved: After adding montmorillonite and sulfuric acid in sequence, heating to a constant temperature, and then adding deionized water for washing; After the cleaning is completed, dodecyl trimethyl ammonium bromide is added thereto for activation to obtain an activated montmorillonite suspension; Add diethylenetriamine, carbon disulfide, sodium sulfide, dithiocarbamate and sodium hydroxide to the activated montmorillonite suspension, continue the reaction, centrifuge and dry to obtain the product.

5. The preparation method according to claim 4, characterized in that: After adding montmorillonite and sulfuric acid in sequence, heat to 90°C-100°C and keep the temperature constant for 3h-5h.

6. The preparation method according to claim 4, characterized in that: The cleaning process includes adding deionized water to wash the precipitate, rinsing until the pH value is 3, and centrifuging and dehydrating.

7. The preparation method according to claim 4, characterized in that: The activation time is 1h-3h.

8. The preparation method according to claim 7, characterized in that: The activation time is 2h.

9. The preparation method according to claim 4, characterized in that: The duration of the continuous reaction is 3h-6h.

10. The preparation method according to claim 9, characterized in that: The duration of the reaction is 4 hours.