Carbon dioxide adsorbent and preparation method thereof

The carbon dioxide adsorbent is prepared by combining cellulose acetate and solvent heating and curing and silicon source hydrolysis and calcining, which solves the problems of difficult molding and recycling of powdered adsorbents, and achieves efficient and stable CO2 adsorption and mechanical properties, which is suitable for industrial applications.

CN119056409APending Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310650139.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing powdered CO2 adsorbents have high pressure drop and difficulty in recycling due to the difficulty of forming, and have high energy consumption and low practicality.

Method used

The silica framework is prepared by combining cellulose acetate and solvent by heating and curing, and the silica skeleton is prepared after washing and calcination of the silicon source, and the ammonization reagent is supported to form a carbon dioxide adsorbent.

Benefits of technology

The prepared carbon dioxide adsorbent has a simple process, low cost, high CO2 adsorption, excellent mechanical properties, stable circulation performance, and is not easy to powder, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056409A_ABST
    Figure CN119056409A_ABST
Patent Text Reader

Abstract

The invention relates to the field of carbon dioxide adsorption, and discloses a carbon dioxide adsorbent and a preparation method thereof, and the preparation method comprises the following steps: (1) firstly adding cellulose acetate into a first solvent, then adding a second solvent for heating, and then introducing into a mold for curing to obtain a cured product; (2) washing the cured product with a third solvent to obtain a shaped product; (3) immersing the integral product in a silicon source, taking out, hydrolyzing in an ammonia gas atmosphere, and calcining to obtain a silicon dioxide skeleton; and (4) loading the ammoniation reagent on the silicon dioxide skeleton to obtain the carbon dioxide adsorbent. The carbon dioxide adsorbent prepared by the preparation method of the carbon dioxide adsorbent provided by the invention has good mechanical properties and high CO2 adsorption capacity, and is stable in cycle performance, not easy to pulverize and wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of carbon dioxide adsorption, and in particular to a carbon dioxide adsorbent and a preparation method thereof. Background Art

[0002] The industrial structure that uses fossil fuels as the main energy source will lead to the emission of a large amount of greenhouse gases, among which CO2, N2O, CH4 and chlorofluorocarbons are the main greenhouse gases that cause the greenhouse effect. Controlling and reducing CO2 emissions from coal-fired power plants is of great significance to alleviating the rapid growth of CO2 concentration in the atmosphere.

[0003] Existing carbon dioxide capture methods mainly include absorption, adsorption and membrane separation. The absorption process is mature, but the energy consumption and corrosive problems are more prominent; membrane separation technology has poor selectivity, short life and high cost. The adsorption method has the advantages of simple operation, easy automation control, low energy consumption and weak corrosiveness. Solid CO2 adsorbents have more significant advantages and have broad application prospects in the field of CO2 emission reduction.

[0004] Currently developed solid CO2 adsorbents are mostly in powder form. In practical applications, due to the small particle size of the powder adsorbent, the bed resistance is large during actual adsorption, resulting in high energy consumption in the adsorption separation process. In addition, the powder adsorbent has the disadvantages of being difficult to recycle and easy to agglomerate, resulting in low practicality.

[0005] Therefore, there is an urgent need to provide a solid CO2 adsorbent with good formability, low production cost, good mechanical properties, high CO2 adsorption capacity, stable cycle performance, and not easy to powderize. Summary of the invention

[0006] The purpose of the present invention is to solve the problems of high bed pressure drop and difficult recovery caused by the difficulty in molding of powdered CO2 adsorption materials, and to provide a carbon dioxide adsorbent and a preparation method thereof.

[0007] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a carbon dioxide adsorbent, wherein the method comprises the following steps:

[0008] (1) first adding cellulose acetate into a first solvent, then adding a second solvent to heat, and then introducing into a mold to cure, to obtain a cured product; wherein the first solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; and the second solvent is selected from one or more of C5-C8 alcohol solvents;

[0009] (2) washing the solidified product with a third solvent to obtain a shaped product; wherein the third solvent is selected from one or more of C1-C4 alcohol solvents;

[0010] (3) immersing the shaping product in a silicon source, taking it out, first hydrolyzing it in an ammonia atmosphere, and then calcining it to obtain a silicon dioxide skeleton;

[0011] (4) loading an aminating agent on the silica skeleton to obtain the carbon dioxide adsorbent; wherein the aminating modifier is selected from one or more of tetraethylenepentamine, triethylenetetramine, pentaethylenehexamine, polyethyleneimine, and polypropyleneimine.

[0012] The second aspect of the present invention provides a carbon dioxide adsorbent prepared by the preparation method described in the first aspect of the present invention.

[0013] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0014] (1) The method for preparing the carbon dioxide adsorbent provided in the present invention has the advantages of simple process and ease of large-scale production, and is suitable for industrial promotion.

[0015] (2) The carbon dioxide adsorbent provided in the present invention has strong plasticity, low cost, high CO2 adsorption capacity, excellent mechanical properties, stable cycle performance, and is not easy to pulverize. It can meet the requirements of industrial flue gas separation and has prospects for practical application. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a scanning electron microscope image of the carbon dioxide adsorbent prepared in Example 1 of the present invention;

[0017] Figure 2 is a scanning electron microscope image of the carbon dioxide adsorbent prepared in Example 2 of the present invention;

[0018] Figure 3 is a scanning electron microscope image of the carbon dioxide adsorbent prepared in Example 3 of the present invention;

[0019] Figure 4 is a scanning electron microscope image of the carbon dioxide adsorbent prepared in Example 4 of the present invention;

[0020] Figure 5 is a scanning electron microscope image of the carbon dioxide adsorbent prepared in Example 5 of the present invention;

[0021] Figure 6 is a scanning electron microscope image of the carbon dioxide adsorbent prepared in Example 6 of the present invention;

[0022] Figure 7This is a graph showing the test results of 50 CO2 adsorption and desorption cycles of the carbon dioxide adsorbent prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0023] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0024] A first aspect of the present invention provides a method for preparing a carbon dioxide adsorbent, wherein the method comprises the following steps:

[0025] (1) first adding cellulose acetate into a first solvent, then adding a second solvent to heat, and then introducing into a mold to cure, to obtain a cured product; wherein the first solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; and the second solvent is selected from one or more of C5-C8 alcohol solvents;

[0026] (2) washing the solidified product with a third solvent to obtain a shaped product; wherein the third solvent is selected from one or more of C1-C4 alcohol solvents;

[0027] (3) immersing the shaping product in a silicon source, taking it out, first hydrolyzing it in an ammonia atmosphere, and then calcining it to obtain a silicon dioxide skeleton;

[0028] (4) loading an aminating agent on the silica skeleton to obtain the carbon dioxide adsorbent; wherein the aminating modifier is selected from one or more of tetraethylenepentamine, triethylenetetramine, pentaethylenehexamine, polyethyleneimine, and polypropyleneimine.

[0029] In step (1),

[0030] In a preferred embodiment, the cellulose acetate has a bound acetic acid content of 50-60%, preferably 54-56%.

[0031] In a preferred embodiment, the usage ratio of the cellulose acetate and the first solvent is 10-50 g:100 mL, preferably 20-40 g:100 mL, and more preferably 25-30 g:100 mL.

[0032] In the present invention, the first solvent is used to dissolve cellulose acetate. The present invention does not specifically limit the dissolution operation of cellulose acetate and the first solvent, and preferably the cellulose acetate is completely dissolved by stirring at room temperature. The room temperature in the present invention has a well-known meaning, which can be 10-35°C.

[0033] In a preferred embodiment, the second solvent is selected from one or more of pentanol, hexanol, and heptanol, preferably one or more of 1-pentanol, 1-hexanol, and 1-heptanol.

[0034] In a preferred embodiment, the volume ratio of the first solvent to the second solvent is 1:0.5-3, preferably 1:0.8-2.5, and more preferably 1:1-2.

[0035] Among them, in the present invention, the second solvent is used to form pores. By controlling the volume ratio of the first solvent and the second solvent, the porosity and skeleton structure of the solid product can be adjusted, thereby changing the density, strength and specific surface area of ​​the carbon dioxide adsorbent, so that the carbon dioxide adsorbent can have both high adsorption effect and good mechanical strength.

[0036] In a preferred embodiment, the second solvent is added dropwise.

[0037] In a preferred embodiment, the heating temperature is 50-80°C, preferably 60-70°C; the heating time is 30-90min, preferably 40-80min. In the present invention, heating can promote the dissolution of the second solvent to obtain a single-phase solution consisting of the first solvent, the second solvent and cellulose acetate.

[0038] In a preferred embodiment, the mold is a polytetrafluoroethylene mold. In the present invention, by injecting the solution containing cellulose acetate, the first solvent and the second solvent into molds of different shapes, the solid phase product can present different macroscopic morphologies. The present invention does not specifically limit the mold, which can be a sheet mold or a cylindrical mold (for example, a cylindrical mold with a diameter of 1-3 cm and a height of 1-5 cm). The specific shape of the mold can be selected according to actual production needs, and the present invention will not repeat them one by one.

[0039] In a preferred embodiment, the curing operating conditions include: first cooling from the heating temperature to room temperature, and then standing at room temperature; preferably, first cooling from 50-80°C to room temperature, and then standing at room temperature for 12-36h; further preferably, first cooling from 60-70°C to room temperature, and then standing at room temperature for 20-30h.

[0040] Among them, in the present invention, after the second solvent is added and heated, it is quickly poured into the mold and then solidified. During the cooling process, cellulose acetate is more easily dissolved in the first solvent, and the first solvent and the second solvent are phase separated due to the concentration difference. According to the different aggregation concentrations of cellulose acetate, a dense phase and a dilute phase can be formed. The viscosity of the dense phase is large, so that the dilute phase cannot escape and stays dispersedly in the dense phase. The position occupied by the dilute phase can eventually form a macroporous channel structure in the solidified product. As the temperature continues to decrease, the cellulose acetate in the dilute phase gradually aggregates into the dense phase, and the cellulose acetate in the dense phase crystallizes and solidifies in the first solvent, thereby forming a solid phase product with a macroporous structure that is interconnected, that is, a cellulose acetate skeleton.

[0041] In step (2),

[0042] In a preferred embodiment, the third solvent is selected from one or more of methanol, ethanol, propanol and butanol.

[0043] In a preferred embodiment, the washing operation includes: first immersing the solidified product in the third solvent at room temperature, and then taking it out for drying.

[0044] Among them, in the present invention, during the process of cellulose acetate aggregation and solidification into a solidified product (i.e., a cellulose acetate skeleton), after the first solvent and the second solvent are separated from the cellulose acetate in turn, a portion of the first solvent and the second solvent are aggregated between the cellulose acetate skeletons. By adding a third solvent, the first solvent and the second solvent can be leached out, thereby obtaining a high-purity shaped macroporous solidified product after drying.

[0045] In a preferred embodiment, the washing is preferably performed 1-5 times. In the present invention, in order to improve the washing effect, the washing operation can be repeated multiple times.

[0046] In step (3),

[0047] In a preferred embodiment, the silicon source is a liquid silicon source selected from one or more of ethyl orthosilicate, methyl orthosilicate, and silicon tetrachloride.

[0048] In a preferred embodiment, the immersion is carried out at room temperature, and the immersion time is 6-48 hours, preferably 12-24 hours. In the present invention, the silicon source can be evenly dispersed on the shaping product by immersion.

[0049] In a preferred embodiment, the hydrolysis is carried out at room temperature for 6-48 hours, preferably 12-24 hours. In the present invention, the silicon source can be hydrolyzed to generate silicon dioxide by placing it under ammonia for a period of time.

[0050] In a preferred embodiment, the heating rate of the calcination is 0.5-7.5°C / min, preferably 2-5°C / min; the calcination temperature is 500-700°C, preferably 500-600°C; and the calcination time is 1-10h, preferably 2-5h.

[0051] In the present invention, a shaped macroporous silica skeleton can be prepared by calcination. In order to improve the calcination effect, a drying treatment can be performed after the ammonia gas is allowed to stand and before calcination.

[0052] In step (4),

[0053] In a preferred embodiment, the weight average molecular weight MW of the polyethyleneimine and / or polypropyleneimine is independently selected from 500-2000, preferably 600-1000.

[0054] In a preferred embodiment, the mass ratio of the silica skeleton to the aminating agent is 1:0.5-5.5, preferably 1:1.5-4.5, and more preferably 1:2-4.

[0055] In a preferred embodiment, the loading operation comprises: mixing the aminating agent and the silica skeleton in a fourth solvent, and then performing rotary evaporation.

[0056] In a preferred embodiment, the fourth solvent is selected from alcohol and / or water, preferably ethanol.

[0057] In a preferred embodiment, the usage ratio of the aminating agent to the fourth solvent is 1 g:5-20 mL, preferably 1 g:10-15 mL.

[0058] In a preferred embodiment, the evaporation temperature of the rotary evaporation is 40-80°C, preferably 50-60°C.

[0059] Among them, in the present invention, as the fourth solvent evaporates, under the action of the concentration difference, the aminating agent enters the interior of the silica skeleton and continuously accumulates on the surface of the silica skeleton, thereby obtaining a carbon dioxide adsorbent. When the carbon dioxide adsorbent is used to adsorb carbon dioxide, a large amount of aminating agent coated on the surface of the silica skeleton can significantly increase the adsorption amount of carbon dioxide, and improve the mechanical strength and recycling performance of the carbon dioxide adsorbent.

[0060] The second aspect of the present invention provides a carbon dioxide adsorbent prepared by the method described in the first aspect of the present invention.

[0061] In a preferred embodiment, the carbon dioxide adsorbent has an axial strength of 3-4.5 MPa and a radial compressive strength of 30-40 N / cm;

[0062] In a preferred embodiment, the specific surface area of ​​the carbon dioxide adsorbent is 200-235m 2 / g.

[0063] The present invention will be described in detail below through examples.

[0064] The combined acid content of cellulose acetate is 55.2%, purchased from Tianjin Xiensi Biochemical Technology Co., Ltd., product number: C-34850+500g; the weight average molecular weight MW of polyethyleneimine is 600, purchased from Innochem, brand Innochem, product number A25622, 10g; the weight average molecular weight MW of polyethyleneimine is 1800, purchased from Innochem, brand Innochem, product number A93927, 25g.

[0065] The polytetrafluoroethylene mold is a perforated polytetrafluoroethylene plate with a plate thickness of 1.5 cm, a hole depth of 1 cm, and a hole diameter of 3 mm.

[0066] Example 1

[0067] (1) First, 56 g of cellulose acetate was added to 200 mL of N,N-dimethylformamide, and stirred until uniform and transparent. Then, 250 mL of 1-pentanol was slowly added dropwise, and the mixture was continued to be stirred and heated to 60° C. After stirring at 60° C. for 50 min, the mixture was injected into a polytetrafluoroethylene mold, cooled naturally to room temperature, and placed at room temperature for 24 h for curing to obtain a cured product;

[0068] (2) soaking the obtained solidified product in ethanol at room temperature to remove 1-pentanol and N,N-dimethylformamide, replacing the ethanol every 8 hours, taking it out after 24 hours for washing, and then drying it at room temperature for 2 days to obtain a solidified product;

[0069] (3) At room temperature, immersing the obtained shaping product in ethyl orthosilicate, taking it out after 24 hours, absorbing the liquid on the surface of the shaping product with filter paper, placing it in an ammonia atmosphere for 24 hours for hydrolysis, and then drying it at 40°C for 2 hours, and then placing it in a muffle furnace, heating it to 550°C at a heating rate of 2°C / min, keeping the temperature constant for 2 hours, and cooling it to room temperature to obtain a silica skeleton;

[0070] (4) 8 g of tetraethylenepentamine was added dropwise to 100 mL of ethanol and stirred for 30 min. Then, 2 g of the above-mentioned silica skeleton was added and stirred for another 30 min. The mixture was then placed in a rotary evaporator and subjected to rotary evaporation at 60° C. to remove the ethanol and obtain a carbon dioxide adsorbent.

[0071] Example 2

[0072] (1) First, 50 g of cellulose acetate was added to 200 mL of N,N-dimethylacetamide, and stirred until uniform and transparent. Then, 300 mL of 1-hexanol was slowly added dropwise, and the mixture was continued to be stirred and heated to 70° C. After stirring at 70° C. for 60 min, the mixture was injected into a polytetrafluoroethylene mold, cooled naturally to room temperature, and placed at room temperature for 24 h for curing to obtain a cured product;

[0073] (2) soaking the obtained solidified product in ethanol at room temperature to remove 1-hexanol and N,N-dimethylacetamide, replacing the ethanol every 8 hours, taking it out after 24 hours for rinsing, and then drying it at room temperature for 2 days to obtain a solidified product;

[0074] (3) At room temperature, immersing the obtained shaping product in methyl orthosilicate, taking it out after 24 hours, absorbing the liquid on the surface of the shaping product with filter paper, placing it in an ammonia atmosphere for 24 hours for hydrolysis, and then drying it at 40°C for 2 hours, and then placing it in a muffle furnace, heating it to 600°C at a heating rate of 5°C / min, keeping it at a constant temperature for 1.5 hours, and cooling it to room temperature to obtain a silica skeleton;

[0075] (4) 8 g of pentaethylenehexamine was added dropwise to 100 mL of ethanol and stirred for 30 min. Then, 3 g of the above-mentioned silica skeleton was added and stirred for another 30 min. The mixture was then placed in a rotary evaporator and subjected to rotary evaporation at 60° C. to remove the ethanol and obtain a carbon dioxide adsorbent.

[0076] Example 3

[0077] (1) First, 60 g of cellulose acetate was added to 200 mL of dimethyl sulfoxide, and stirred until uniform and transparent, and then 350 mL of 1-heptanol was slowly added dropwise, and the mixture was continued to be stirred and heated to 65° C. After stirring at 65° C. for 70 min, the mixture was injected into a polytetrafluoroethylene mold, cooled naturally to room temperature, and placed at room temperature for 24 h for curing to obtain a cured product;

[0078] (2) soaking the obtained solidified product in ethanol at room temperature to remove 1-heptanol and dimethyl sulfoxide, replacing the ethanol every 8 hours, taking it out after 24 hours for rinsing, and then drying it at room temperature for 2 days to obtain a solidified product;

[0079] (3) At room temperature, immersing the obtained shaping product in silicon tetrachloride, taking it out after 24 hours, absorbing the liquid on the surface of the shaping product with filter paper, placing it in an ammonia atmosphere for 24 hours for hydrolysis, and then drying it at 40°C for 2 hours, and then placing it in a muffle furnace, heating it to 500°C at a heating rate of 3°C / min, keeping the temperature constant for 4 hours, and cooling it to room temperature to obtain a silica skeleton;

[0080] (4) 8 g of triethylenetetramine was added dropwise to 100 mL of ethanol and stirred for 30 min. Then, 4 g of the above-mentioned silica skeleton was added and stirred for another 30 min. The mixture was then placed in a rotary evaporator and subjected to rotary evaporation at 60° C. to remove the ethanol and obtain a carbon dioxide adsorbent.

[0081] Example 4

[0082] The same as Example 1, except that in step (1), the amount of 1-hexanol added is 100 mL.

[0083] Example 5

[0084] The same as Example 1, except that in step (4), tetraethylenepentamine is replaced by polyethyleneimine with a weight average molecular weight of 600.

[0085] Example 6

[0086] The same as Example 1, except that in step (4), tetraethylenepentamine is replaced by polyethyleneimine with a weight average molecular weight of 1800.

[0087] Test Example 1

[0088] The microscopic appearance of the carbon dioxide adsorbent prepared in Examples 1-6 was characterized, and the results were as follows: Figure 1-6 shown.

[0089] Among them, Figure 1-6 It can be seen that the carbon dioxide adsorbents prepared in Examples 1-6 are all composed of a skeleton and a pore structure that penetrates each other between the skeletons. The rich pore structure in the carbon dioxide adsorbent can not only provide abundant attachment sites for the aminating reagent, but also provide a flow channel for the airflow, which can reduce the adsorbent bed resistance during carbon dioxide adsorption and extend the operation cycle.

[0090] Test Example 2

[0091] The axial strength, radial compressive strength and specific surface area of ​​the carbon dioxide adsorbent prepared in Examples 1-6 were tested. The test results are shown in Table 1:

[0092] Table 1

[0093] Axial strength / MPa Radial compressive strength / N / cm <![CDATA[Specific surface area / m 2 / g]]> Example 1 3.2 34.5 227.74 Example 2 3.1 33.6 231.56 Example 3 3.5 35.9 225.95 Example 4 4.2 38.3 207.61 Example 5 3.1 34.2 225.23 Example 6 3.1 34.3 221.74

[0094] Among them, it can be seen from Table 1 that the carbon dioxide adsorbent prepared by the method of the present invention can take into account both good mechanical properties and a large specific surface area.

[0095] By comparing Example 1 and Example 4, it can be seen that when the amount of the second solvent is large, more pores are formed during the curing process, which leads to a slender skeleton of the cured product, increased porosity, and thus good adsorption performance. When the amount of the second solvent is small, the skeleton of the silica skeleton is coarse, the pore structure is small, the material is relatively compact, the mechanical properties are enhanced, but the specific surface area is reduced. When the volume ratio of the first solvent to the second solvent is controlled between 1:1-2, a high specific surface area and good mechanical strength can be achieved.

[0096] Test Example 3

[0097] The carbon dioxide adsorption performance of the carbon dioxide adsorbent prepared in Examples 1-6 was tested, and the specific test method is as follows:

[0098] 20 mg of the carbon dioxide adsorbent prepared in Examples 1-6 was respectively placed in a thermogravimetric crucible (thermogravimetric model: Netzsch STA 449F5), first heated to 100 ° C in a nitrogen atmosphere, kept at this temperature for 20 min, and the water and carbon dioxide adsorbed by the adsorbent were removed. Then the temperature was lowered to 75 ° C, and the flow rate was 100 mL min -1 The simulated flue gas (the content of carbon dioxide is 12v%, the content of nitrogen is 88v%), adsorbed for 1h. The carbon dioxide adsorption capacity per unit mass of the adsorbent (mg / g) was calculated according to the weight increase of the carbon dioxide adsorbent. The test results are shown in Table 2:

[0099] Table 2

[0100]

[0101] Among them, it can be seen from the test results in Table 2 that the carbon dioxide adsorbent prepared in the present invention has an adsorption capacity of carbon dioxide of more than 200 mg / g under the test conditions.

[0102] By comparing Examples 5 and 6, it can be seen that the adsorption performance of the carbon dioxide adsorbent for carbon dioxide decreases with the increase of the weight average molecular weight of polyethyleneimine. The reason may be that polyethyleneimine is not a linear structure, but a branched structure. The larger the molecular weight, the longer the branch, resulting in a decrease in the number of primary amines in the polyethyleneimine structure, thereby causing the phenomenon that the carbon dioxide adsorption amount decreases with the increase of the weight average molecular weight of polyethyleneimine.

[0103] Test Example 4

[0104] The adsorption cycle performance of the carbon dioxide adsorbent prepared in Examples 1-6 was tested, and the test method was as follows:

[0105] 2.0 g of the carbon dioxide adsorbent prepared in Examples 1-6 was respectively loaded into a quartz tube of a fixed bed reactor, the inner diameter of the quartz tube being 16 mm; -1 The simulated flue gas (the content of carbon dioxide is 12v%, the content of nitrogen is 88v%) was introduced at a flow rate of 1.5 ℃, and the adsorption was stopped at 75℃ for 1h. After cooling to room temperature, the carbon dioxide adsorbent was taken out and weighed to calculate the adsorption amount of carbon dioxide. The weighed carbon dioxide adsorbent was then put back into the fixed bed reactor and heated at 100mL min -1 High-purity nitrogen was introduced at a flow rate of 100°C and regenerated at a constant temperature of 100°C for 1 hour to obtain a regenerated carbon dioxide adsorbent; the above adsorption-regeneration operation was repeated on the regenerated carbon dioxide adsorbent for a total of 50 times. The adsorption effect of the 50th time is shown in Table 3:

[0106] Table 3

[0107]

[0108] It can be seen from Table 3 that after the carbon dioxide adsorbent material provided by the present invention repeats the adsorption-regeneration operation 50 times, the adsorption amount of carbon dioxide can be maintained above 175 mg / g.

[0109] In the process of testing the adsorption cycle performance of the carbon dioxide adsorbent prepared in Example 1, the test results were recorded every 5 times. Figure 4 As shown. Figure 4 It can be seen that the carbon dioxide adsorbent prepared in Example 1 has very good stability in the adsorption amount of carbon dioxide during 50 adsorption-regeneration operations.

[0110] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a carbon dioxide adsorbent, characterized in that: The method comprises the following steps: (1) first adding cellulose acetate into a first solvent, then adding a second solvent to heat, and then introducing into a mold to cure, to obtain a cured product; wherein the first solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; and the second solvent is selected from one or more of C5-C8 alcohol solvents; (2) washing the solidified product with a third solvent to obtain a shaped product; wherein the third solvent is selected from one or more of C1-C4 alcohol solvents; (3) immersing the shaping product in a silicon source, taking it out, first hydrolyzing it in an ammonia atmosphere, and then calcining it to obtain a silicon dioxide skeleton; (4) loading an aminating agent on the silica skeleton to obtain the carbon dioxide adsorbent; wherein the aminating modifier is selected from one or more of tetraethylenepentamine, triethylenetetramine, pentaethylenehexamine, polyethyleneimine, and polypropyleneimine.

2. The preparation method according to claim 1, wherein The cellulose acetate has a combined acetic acid content of 50-60%, preferably 54-56%; Preferably, the usage ratio of the cellulose acetate and the first solvent is 10-50 g:100 mL, preferably 20-40 g:100 mL, and more preferably 25-30 g:100 mL.

3. The preparation method according to claim 1 or 2, wherein The second solvent is selected from one or more of pentanol, hexanol, and heptanol, preferably one or more of 1-pentanol, 1-hexanol, and 1-heptanol; Preferably, the volume ratio of the first solvent to the second solvent is 1:0.5-3, preferably 1:0.8-2.5, and more preferably 1:1-2; Preferably, the second solvent is added dropwise; Preferably, the heating temperature is 50-80°C, preferably 60-70°C; the heating time is 30-90min, preferably 40-80min.

4. The preparation method according to claim 3, wherein The curing operation conditions include: first cooling from the heating temperature to room temperature, and then standing at room temperature; Preferably, first cool from 50-80°C to room temperature, and then stand at room temperature for 12-36h; More preferably, the mixture is first cooled from 60-70° C. to room temperature, and then allowed to stand at room temperature for 20-30 hours.

5. The preparation method according to any one of claims 1 to 4, wherein: The third solvent is selected from one or more of methanol, ethanol, propanol, and butanol; Preferably, the washing operation comprises: firstly immersing the solidified product in the third solvent at room temperature, and then taking it out for drying.

6. The preparation method according to any one of claims 1 to 5, wherein: The silicon source is a liquid silicon source, preferably one or more selected from ethyl orthosilicate, methyl orthosilicate, and silicon tetrachloride; Preferably, the immersion is carried out at room temperature, and the immersion time is 6-48h, preferably 12-24h; Preferably, the hydrolysis is carried out at room temperature, and the hydrolysis time is 6-48h, preferably 12-24h; Preferably, the heating rate of the calcination is 0.5-7.5°C / min, preferably 2-5°C / min; the calcination temperature is 500-700°C, preferably 500-600°C; and the calcination time is 1-10h, preferably 2-5h.

7. The preparation method according to any one of claims 1 to 6, wherein: The mass ratio of the silica skeleton to the aminating agent is 1:0.5-5.5, preferably 1:1.5-4.5, and more preferably 1:2-4.

8. The preparation method according to any one of claims 1 to 7, wherein: The loading operation includes: mixing the aminating agent and the silica skeleton in a fourth solvent, and then performing rotary evaporation; Preferably, the fourth solvent is selected from alcohol and / or water, preferably ethanol; Preferably, the usage ratio of the aminating agent and the fourth solvent is 1 g: 5-20 mL, preferably 1 g: 10-15 mL; Preferably, the evaporation temperature of the rotary evaporation is 40-80°C, preferably 50-60°C.

9. The carbon dioxide adsorbent prepared by the preparation method according to any one of claims 1 to 8.

10. The carbon dioxide adsorbent according to claim 9, wherein The carbon dioxide adsorbent has an axial strength of 3-4.5 MPa and a radial compressive strength of 30-40 N / cm; Preferably, the specific surface area of ​​the carbon dioxide adsorbent is 200-235m 2 / g.