Ni3ZnC0.7 atC-g-C3N4 photocatalyst as well as preparation method and application thereof

By loading Ni3ZnC0.7@C nanoparticles on g-C3N4, a carbon-coated spherical nanoparticle structure is formed, and the problem of insufficient catalytic activity of existing photocatalysts is solved, and efficient photocatalytic hydrogen production effect is achieved and production is reduced. cost.

CN119056481AActive Publication Date: 2024-12-03SHAANXI UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411308711.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

The existing photocatalysts have limited catalytic activity in the process of photocatalytic water cracking and hydrogen production, and the commonly used cocatalysts are costly, making it difficult to achieve efficient and low-cost photocatalytic performance improvement.

Method used

G-C3N4 nanosheets were prepared by one-step calcination method, and combined with hydrothermal method and solid-phase sintering method, Ni3ZnC0.7@C nanoparticles were loaded on g-C3N4 to form a carbon-coated spherical nanoparticle structure, increasing the ratio Surface area and active sites promote separation and transport of photogenerated charges.

Benefits of technology

The photocatalytic hydrogen production efficiency is improved, the preparation cost is reduced, the efficient photocatalytic performance is achieved, and the preparation conditions are simple and easy to control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056481A_ABST
    Figure CN119056481A_ABST
Patent Text Reader

Abstract

The invention discloses a Ni3ZnC0.7 atC / g-C3N4 photocatalyst and a preparation method and application thereof.The preparation process comprises the steps that a hydrothermal method and a solid-phase sintering method are combined, firstly, porous g-C3N4 nanosheets are prepared through a calcination method, and the specific surface area of a product and active sites during photocatalytic hydrogen production are increased; then preparing a NiZn-LDH / g-4 precursor by adopting a hydrothermal method, further carbonizing to obtain a C-coated Ni3ZnC0.7 material, and finally preparing the Ni3ZnC0.7 (at) C / g-C3N4 composite photocatalytic material with high hydrogen production efficiency by adopting low-temperature annealing. Preparation conditions are simple and easy to control, and production cost is low; ni3ZnC0.7 and C are integrated through interface electronic engineering, so that Ni3ZnC0.7 and C form a heterostructure of carbon-coated spherical nanoparticles, agglomeration of the nanoparticles is inhibited, the specific surface area and active sites of the Ni3ZnC0.7 and C / g-C3N4 composite photocatalyst are increased, a carbon shell on the surface provides a rapid charge transfer way for rapid migration of electrons and ions in the electrochemical process, and the specific surface area of the Ni3ZnC0.7 and C / g-C3N4 composite photocatalyst is increased. The separation and transmission of photo-generated charges can be effectively promoted, so that the hydrogen production efficiency is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional materials, and relates to a photocatalyst, and specifically to a Ni3ZnC 0.7 @C / g-C3N4 photocatalyst, its preparation method and application. Background Art

[0002] As the energy crisis intensifies, humans have begun to seek green, environmentally friendly and sustainable energy to replace fossil fuels. Hydrogen is considered an ideal alternative energy source because of its cleanness, wide sources and high combustion calorific value. Among various hydrogen production methods, photocatalytic water splitting is considered to be a very promising method. In order to promote the industrialization of photocatalytic hydrogen production technology, the development of efficient photocatalysts remains the focus of current research. Graphitic carbon nitride (CN) is a visible light responsive photocatalyst with a unique two-dimensional structure, excellent chemical stability and adjustable electronic structure. However, due to the rapid recombination of electron-hole pairs generated by light, the photocatalytic activity of pure CN is limited. In order to enhance the photocatalytic performance of CN, people have developed a variety of methods to improve the photocatalytic activity of carbon nitride. At present, using g-C3N4 nanosheets as a matrix, the development of new composite photocatalytic materials is an important way to improve the performance of photocatalytic hydrogen production, which is of great significance for the further development of new composite photocatalytic materials. In the study of visible light photocatalytic hydrogen production of g-C3N4 semiconductor, a co-catalyst is needed to further improve the catalytic activity of the sample. So far, most co-catalysts are rare and expensive metals with high costs. Therefore, it is of great significance to develop co-catalysts with abundant content, low cost and excellent performance to improve the photocatalytic activity of g-C3N4.

[0003] Transition metal carbides (TMC) (such as Fe3C, Co3C, Ni3C, etc.) are considered to be a typical class of metal interstitial compounds. Studies have shown that interstitial C atoms can expand the lattice distance between transition metals in TMCs, leading to the contraction of the transition metal d-band center and the increase of the state density near the Fermi level, which will give TMC unique surface adsorption properties, and the electronic structure is significantly similar to Pt. Compared with single metal carbides, bimetallic carbides have the advantages of adjustable active sites, adjustable electronic structure, and adjustable coordination environment, and have broad application prospects in the field of energy conversion and storage. Among them, Ni3ZnC 0.7 Due to its excellent perovskite-like metallic conductivity and structural stability, Ni3ZnC can be used as a potential bimetallic carbide catalyst for hydrogen evolution reaction (HER). However, due to insufficient catalytic active sites and unoptimized electronic and electrical structures, Ni3ZnC 0.7 The catalytic performance of Ni3ZnC is not ideal. 0.7The preparation of nanoparticles usually requires a relatively harsh high-temperature pyrolysis process, which will inevitably lead to the agglomeration or coarsening of the nanoparticles, which largely reduces the exposure of active sites. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention aims to provide a Ni3ZnC 0.7 @C / g-C3N4 photocatalyst and its preparation method and application, Ni3ZnC 0.7 The heterogeneous structure in which @C nanoparticles are uniformly loaded on g-C3N4 nanosheets has a large specific surface area and multiple active sites, high hydrogen production efficiency, simple and easy-to-control preparation conditions, and low production cost.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A Ni3ZnC 0.7 The preparation method of @C / g-C3N4 photocatalyst comprises the following steps:

[0007] Step 1: Prepare nano-sheet g-C3N4 by a one-step calcination method;

[0008] Step 2, nickel chloride, zinc acetate, urea and acetylacetone are mixed in a molar ratio of (1-3):(1-2):(1-5):(0.1-0.6) to obtain a mixed powder, and then the mixed powder and the nano-sheet g-C3N4 prepared in step 1 are mixed in a mass ratio of 1:(1-6), water and ethylene glycol mixed solution are added, ultrasonic treatment is performed, and then the mixture is stirred until uniformly dispersed, and then poured into the lining of a reactor, placed in a vacuum drying oven at 100-160°C for 10-16h, and the reactor is taken out after the temperature in the oven drops to room temperature, centrifuged, washed, and dried to obtain NiZn-LDH / g-C3N4;

[0009] Step 3: Mix the NiZn-LDH / g-C3N4 prepared in step 2 with melamine in a mass ratio of (0.5-4):(1-10), grind and spread on a porcelain boat and then place it in a tube furnace. In an argon atmosphere, heat the tube furnace to 500-700°C at a rate of 5-10°C / min, keep warm for 2-4h, and after the product is cooled, take out and grind to obtain Ni3ZnC 0.7 @C promoter;

[0010] Step 4: First, the Ni3ZnC prepared in step 3 0.7The @C co-catalyst and the nano-sheet g-C3N4 prepared in step 1 are mixed in a mass ratio of (0.5-1):(5-10) and placed in a tube furnace. The tube furnace is heated to 200-400°C at a rate of 2-5°C / min under an argon atmosphere and kept warm for 1-3h. After the product is cooled, it is taken out to obtain Ni3ZnC 0.7 @C / g-C3N4 photocatalyst.

[0011] The present invention also has the following technical features:

[0012] Preferably, the specific steps of preparing nano-sheet g-C3N4 by the one-step calcination method described in step 1 include:

[0013] Urea and dicyandiamide are sequentially placed in a beaker containing a sulfuric acid solution in a mass ratio of (1-5):(1-3), and stirred for 1-3 hours. Finally, the mixed solution is placed in a water bath and heated at 60-80°C for 1-6 hours. After the reaction is completed, the cooled reaction solution is poured out, centrifuged, and washed to obtain solid A.

[0014] The volume ratio of 1M concentrated sulfuric acid to ultrapure water in the sulfuric acid solution is (1-2):(2-5);

[0015] Spread solid A on a porcelain boat, place it in a tube furnace under air atmosphere, heat it to 450-600°C at a rate of 2-10°C / min, and keep it warm for 1-4h. After calcination, the sample is naturally cooled in the furnace and ground to obtain yellow powder B, i.e., flaky g-C3N4.

[0016] Preferably, the volume ratio of ethylene glycol to ultrapure water in the water and ethylene glycol mixture described in step 2 is (1-2):(3-5).

[0017] Preferably, the ultrasonic treatment time in step 2 is 30-120 min.

[0018] Preferably, the stirring in step 2 is stirring on a magnetic stirrer for 60-150 min.

[0019] Preferably, the washing is performed with deionized water and anhydrous ethanol for 3-5 times respectively.

[0020] Preferably, the drying in step 2 is performed in a vacuum drying oven for 10-20 hours.

[0021] Preferably, the grinding is performed in a mortar for 30-120 min.

[0022] The present invention also protects a Ni3ZnC prepared by the method as described above. 0.7 @C / g-C3N4 photocatalyst and its application in photocatalytic hydrogen production.

[0023] Compared with the prior art, the present invention has the following technical effects:

[0024] The present invention is used to prepare Ni3ZnC 0.7 In the process of preparing C / g-C3N4 composite photocatalytic materials, the hydrothermal method and solid phase sintering method were combined. The g-C3N4 nanosheets were first prepared by calcination, and then the NiZn-LDH / g-C3N4 precursor was prepared by hydrothermal method, which was further carbonized to obtain C-coated Ni3ZnC 0.7 Materials, Ni3ZnC through interface electronic engineering 0.7 Integrated with C, Ni3ZnC 0.7 @C forms a heterogeneous structure of carbon-coated spherical nanoparticles, which is beneficial to inhibit the agglomeration of nanoparticles and is used to increase the Ni3ZnC 0.7 The specific surface area and active sites of @C / g-C3N4 composite photocatalysts, the carbon shell on the surface provides a fast charge transfer pathway for the rapid migration of electrons and ions in the electrochemical process, which can effectively promote the separation and transmission of photogenerated charges; finally, Ni3ZnC with high hydrogen production efficiency was prepared by low temperature annealing. 0.7 @C / g-C3N4 composite photocatalytic material; the preparation conditions are simple and easy to control, and the production cost is low;

[0025] The porous g-C3N4 nanosheets prepared by the present invention further increase the specific surface area of ​​the product and the active sites during photocatalytic hydrogen production, thereby effectively improving the hydrogen production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Ni3ZnC prepared in Example 1 0.7 @X-ray diffraction analysis diagram of C / g-C3N4, where the horizontal axis is the 2θ angle and the vertical axis is the diffraction peak intensity;

[0027] Figure 2 Ni3ZnC prepared in Example 1 0.7 @C / g-C3N4 scanning image at 5μm;

[0028] Figure 3 Ni3ZnC prepared in Example 1 0.7 @C / g-C3N4 hydrogen evolution performance diagram. DETAILED DESCRIPTION

[0029] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.

[0030] Embodiment 1:

[0031] Step 1, urea and dicyandiamide are placed in a beaker containing sulfuric acid solution in a mass ratio of 5:3, wherein the volume ratio of 1M concentrated sulfuric acid to ultrapure water is 1:3, and then stirred for 2 hours, and finally the mixed solution is placed in a water bath and heated for 4 hours at a temperature of 70°C. After the reaction is completed, the cooled reaction solution is poured out and centrifuged, and washed three times with deionized water and anhydrous ethanol respectively, to obtain solid A;

[0032] 4 g of solid A was spread in a porcelain boat and calcined at 550°C in air atmosphere for 4 h at a heating rate of 5°C / min.

[0033] After calcination, the sample was naturally cooled in the furnace and ground in a mortar for 60 min to obtain yellow powder B, i.e., flaky g-C3N4;

[0034] Step 2: nickel chloride, zinc acetate, urea and acetylacetone are prepared in a molar ratio of 3:1:4:0.4, and then mixed with powder B in a ratio of 1:5 to obtain mixed powder C, and then 50 mL of ethylene glycol solution is added, wherein the volume ratio of ethylene glycol to ultrapure water is 2:3, first ultrasonically stir for 120 minutes, then stir on a magnetic stirrer for 100 minutes, and then quickly pour the mixed solution into a 150 mL reactor liner;

[0035] The working temperature of the vacuum drying oven was set to 140°C. When the temperature in the drying oven rose to the set temperature, the sealed reactor was placed in the oven and kept warm for 14 hours. After the temperature in the oven dropped to room temperature, the reactor was taken out and cooled. The cooled reaction solution was poured out and centrifuged, and washed three times with deionized water and anhydrous ethanol respectively to obtain a precipitate, which was then placed in a vacuum drying oven at 80°C and dried for 10 hours to obtain solid D, namely NiZn-LDH / g-C3N4.

[0036] Step 3: Mix solid D and melamine in a mass ratio of 2:5, and grind them in a mortar for 30 minutes to obtain powder E. Spread powder E flatly on a porcelain boat and place it in a tube furnace. Then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted. Then, heat the tube furnace to 550°C at a heating rate of 10°C / min, and then keep it warm for 2 hours. After the product is cooled, take it out and grind it for 60 minutes to obtain powder F, that is, Ni3ZnC 0.7 @C promoter;

[0037] Step 4: First, mix powder F and powder B in a mass ratio of 1:5, then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted, then heat the tube furnace to 300°C at a heating rate of 2°C / min, and then keep it warm for 2h. After the product is cooled, take it out to obtain Ni3ZnC 0.7@C / g-C3N4 photocatalyst;

[0038] The LabSolar 6A equipment was used to measure the Ni3ZnC 0.7 @C / g-C3N4 was used to test the photocatalytic effect. The specific test process includes weighing 30 mg of the composite photocatalyst and 15 mL of isopropanol, placing them in a glass reaction container filled with 85 mL of deionized water, and irradiating them with light for 4 hours.

[0039] Figure 1 Ni3ZnC prepared in Example 1 0.7 @C / g-C3N4 X-ray diffraction analysis diagram, where the horizontal axis is the 2θ angle and the vertical axis is the diffraction peak intensity; 13° and 27° correspond to the (100) crystal plane and (002) crystal plane of g-C3N4 respectively, and Ni3ZnC 0.7 @C / g-C3N4 can also accurately correspond to Ni3ZnC 0.7 PDF#28-0713 and CPDF#26-1077, showing the successful preparation of Ni3ZnC 0.7 @C / g-C3N4 photocatalyst.

[0040] Figure 2 Ni3ZnC prepared in this comparative example 2 0.7 @C / g-C3N4 scanning image at 5μm. Among them, Ni3ZnC 0.7 @C presents a spherical nanoparticle structure and is evenly distributed on the g-C3N4 nanosheets.

[0041] Figure 3 Ni3ZnC prepared in Example 1 0.7 @C / g-C3N4 hydrogen evolution performance diagram. As shown in the figure, adding Ni3ZnC 0.7 After @C, the hydrogen evolution activity of g-C3N4 was significantly improved, and the amount of hydrogen evolution reached 643.075 μmol / g within four hours.

[0042] Embodiment 2:

[0043] Step 1, urea and dicyandiamide are placed in a beaker containing sulfuric acid solution in a mass ratio of 1:1, wherein the volume ratio of 1M concentrated sulfuric acid to ultrapure water is 1:2, and then stirred for 1 hour, and finally the mixed solution is placed in a water bath and heated for 6 hours at a temperature of 60°C. After the reaction is completed, the cooled reaction solution is poured out and centrifuged, and washed four times with deionized water and anhydrous ethanol respectively, to obtain solid A;

[0044] 2 g of solid A was spread in a porcelain boat and calcined at 600 °C in air atmosphere for 2 h at a heating rate of 6 °C / min.

[0045] After calcination, the sample was naturally cooled in the furnace and ground in a mortar for 30 min to obtain yellow powder B, i.e., flaky g-C3N4;

[0046] Step 2: nickel chloride, zinc acetate, urea and acetylacetone are prepared in a molar ratio of 2:1:3:0.5, and then mixed with powder B in a ratio of 1:6 to obtain mixed powder C, and then 60 mL of ethylene glycol solution is added, wherein the volume ratio of ethylene glycol to ultrapure water is 1:5, first ultrasonically stir for 60 minutes, then stir on a magnetic stirrer for 120 minutes, and then quickly pour the mixed solution into a 150 mL reactor liner;

[0047] The working temperature of the vacuum drying oven was set to 160°C. When the temperature in the drying oven rose to the set temperature, the sealed reactor was placed in the oven and kept warm for 10 hours. After the temperature in the oven dropped to room temperature, the reactor was taken out and cooled. The cooled reaction solution was poured out and centrifuged, and washed four times with deionized water and anhydrous ethanol respectively to obtain a precipitate, which was then placed in a vacuum drying oven at 60°C and dried for 15 hours to obtain solid D, namely NiZn-LDH / g-C3N4.

[0048] Step 3: Mix solid D and melamine at a mass ratio of 1:5, and grind them in a mortar for 60 minutes to obtain powder E. Spread powder E flatly on a porcelain boat and place it in a tube furnace. Then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted. Then, heat the tube furnace to 600°C at a heating rate of 10°C / min, and then keep it warm for 2 hours. After the product is cooled, take it out and grind it for 30 minutes to obtain powder F, that is, Ni3ZnC 0.7 @C promoter;

[0049] Step 4: First, mix powder F and powder B in a mass ratio of 0.6:5, then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted, then heat the tube furnace to 250°C at a heating rate of 2°C / min, and then keep it warm for 2h. After the product is cooled, take it out to obtain Ni3ZnC 0.7 @C / g-C3N4 photocatalyst;

[0050] The LabSolar 6A equipment was used to measure the Ni3ZnC 0.7 @C / g-C3N4 was used to test the photocatalytic effect. The specific test process includes weighing 30 mg of the composite photocatalyst and 15 mL of isopropanol, placing them in a glass reaction container filled with 85 mL of deionized water, and irradiating them with light for 4 hours.

[0051] Embodiment 3:

[0052] Step 1, urea and dicyandiamide are placed in a beaker containing sulfuric acid solution in a mass ratio of 2:3, wherein the volume ratio of 1M concentrated sulfuric acid to ultrapure water is 1:2, and then stirred for 2 hours, and finally the mixed solution is placed in a water bath and heated for 3 hours at a temperature of 80°C. After the reaction is completed, the cooled reaction solution is poured out and centrifuged, and washed five times with deionized water and anhydrous ethanol respectively, to obtain solid A;

[0053] 3 g of solid A was spread in a porcelain boat and calcined at 500 °C in air atmosphere for 2 h at a heating rate of 2 °C / min.

[0054] After calcination, the sample was naturally cooled in the furnace and ground in a mortar for 60 min to obtain yellow powder B, i.e., flaky g-C3N4;

[0055] Step 2: nickel chloride, zinc acetate, urea and acetylacetone are prepared in a molar ratio of 3:2:4:0.6, and then mixed with powder B in a ratio of 1:4 to obtain mixed powder C, and then 50 mL of ethylene glycol solution is added, wherein the volume ratio of ethylene glycol to ultrapure water is 2:5, first ultrasonically stir for 90 minutes, then place on a magnetic stirrer and stir for 120 minutes, and then quickly pour the mixed solution into a 150 mL reactor liner;

[0056] The working temperature of the vacuum drying oven was set to 140°C. When the temperature in the drying oven reached the set temperature, the sealed reactor was placed in the oven and kept warm for 12 hours. After the temperature in the oven dropped to room temperature, the reactor was taken out and cooled. The cooled reaction solution was poured out and centrifuged, and washed five times with deionized water and anhydrous ethanol respectively to obtain a precipitate, which was then placed in a vacuum drying oven and dried for 12 hours to obtain solid D, namely NiZn-LDH / g-C3N4;

[0057] Step 3: Mix solid D and melamine at a mass ratio of 2:5, and grind them in a mortar for 60 minutes to obtain powder E. Spread powder E flatly and place it in a porcelain boat in a tube furnace, then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted. Then, heat the tube furnace to 700°C at a heating rate of 10°C / min, and then keep it warm for 2 hours. After the product is cooled, take it out and grind it for 30 minutes to obtain powder F, that is, Ni3ZnC 0.7 @C promoter;

[0058] Step 4: First, mix powder F and powder B in a mass ratio of 1:5, then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted, then heat the tube furnace to 400°C at a heating rate of 5°C / min, and then keep it warm for 2h. After the product is cooled, take it out to obtain Ni3ZnC 0.7@C / g-C3N4 photocatalyst;

[0059] The LabSolar 6A equipment was used to measure the Ni3ZnC 0.7 @C / g-C3N4 was used to test the photocatalytic effect. The specific test process includes weighing 30 mg of the composite photocatalyst and 15 mL of isopropanol, placing them in a glass reaction container filled with 85 mL of deionized water, and irradiating them with light for 4 hours.

[0060] Embodiment 4:

[0061] Step 1, urea and dicyandiamide are placed in a beaker containing sulfuric acid solution in a mass ratio of 5:1, wherein the volume ratio of 1M concentrated sulfuric acid to ultrapure water is 2:5, and then stirred for 3 hours, and finally the mixed solution is placed in a water bath and heated for 1 hour at a temperature of 80°C. After the reaction is completed, the cooled reaction solution is poured out and centrifuged, and washed five times with deionized water and anhydrous ethanol respectively, to obtain solid A;

[0062] 3 g of solid A was spread in a porcelain boat and calcined at 450°C in air atmosphere for 1 h at a heating rate of 10°C / min.

[0063] After calcination, the sample was naturally cooled in the furnace and ground in a mortar for 120 min to obtain yellow powder B, i.e., flaky g-C3N4;

[0064] Step 2: nickel chloride, zinc acetate, urea and acetylacetone are prepared in a molar ratio of 1:1.5:1:0.1, and then mixed with powder B in a ratio of 1:1 to obtain mixed powder C, and then 50 mL of ethylene glycol solution is added, wherein the volume ratio of ethylene glycol to ultrapure water is 1.5:4, first ultrasonically stir for 30 minutes and then stir on a magnetic stirrer for 60 minutes, and then quickly pour the mixed solution into a 150 mL reactor liner;

[0065] The working temperature of the vacuum drying oven was set to 100°C. When the temperature in the drying oven reached the set temperature, the sealed reactor was placed in the oven and kept warm for 16 hours. After the temperature in the oven dropped to room temperature, the reactor was taken out and cooled. The cooled reaction solution was poured out and centrifuged, and washed five times with deionized water and anhydrous ethanol respectively to obtain a precipitate, which was then placed in a vacuum drying oven at 60°C and dried for 20 hours to obtain solid D, namely NiZn-LDH / g-C3N4;

[0066] Step 3: Mix solid D and melamine at a mass ratio of 0.5:10, and grind them in a mortar for 120 minutes to obtain powder E. Spread powder E flatly and place it in a porcelain boat in a tube furnace, then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted. Then, heat the tube furnace to 650°C at a heating rate of 5°C / min, and then keep it warm for 3 hours. After the product is cooled, take it out and grind it for 60 minutes to obtain powder F, that is, Ni3ZnC 0.7 @C promoter;

[0067] Step 4: First, mix powder F and powder B in a mass ratio of 0.5:10, then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted, then heat the tube furnace to 200°C at a heating rate of 3°C / min, and then keep it warm for 1h. After the product is cooled, take it out to obtain Ni3ZnC 0.7 @C / g-C3N4 photocatalyst;

[0068] The LabSolar 6A equipment was used to measure the Ni3ZnC 0.7 @C / g-C3N4 was used to test the photocatalytic effect. The specific test process includes weighing 30 mg of the composite photocatalyst and 15 mL of isopropanol, placing them in a glass reaction container filled with 85 mL of deionized water, and irradiating them with light for 4 hours.

[0069] Embodiment 5:

[0070] Step 1, urea and dicyandiamide are placed in a beaker containing sulfuric acid solution in a mass ratio of 3:2, wherein the volume ratio of 1M concentrated sulfuric acid to ultrapure water is 1.5:2, and then stirred for 2 hours, and finally the mixed solution is placed in a water bath and heated for 3 hours at a temperature of 80°C. After the reaction is completed, the cooled reaction solution is poured out and centrifuged, and washed five times with deionized water and anhydrous ethanol respectively, to obtain solid A;

[0071] 3 g of solid A was spread in a porcelain boat and calcined at 450°C in air atmosphere for 1 h at a heating rate of 10°C / min.

[0072] After calcination, the sample was naturally cooled in the furnace and ground in a mortar for 80 min to obtain yellow powder B, i.e., flaky g-C3N4;

[0073] Step 2: nickel chloride, zinc acetate, urea and acetylacetone are prepared in a molar ratio of 3:1:5:0.2, and then mixed with powder B in a ratio of 1:3 to obtain mixed powder C, and then 50 mL of ethylene glycol solution is added, wherein the volume ratio of ethylene glycol to ultrapure water is 1:3, first ultrasonically stir for 90 minutes, then stir on a magnetic stirrer for 150 minutes, and then quickly pour the mixed solution into a 150 mL reactor liner;

[0074] The working temperature of the vacuum drying oven was set to 120°C. When the temperature in the drying oven reached the set temperature, the sealed reactor was placed in the oven and kept warm for 12 hours. After the temperature in the oven dropped to room temperature, the reactor was taken out and cooled. The cooled reaction solution was poured out and centrifuged, and washed five times with deionized water and anhydrous ethanol respectively to obtain a precipitate, which was then placed in a vacuum drying oven at 80°C and dried for 12 hours to obtain solid D, namely NiZn-LDH / g-C3N4;

[0075] Step 3: Mix solid D and melamine in a mass ratio of 4:1, and grind them in a mortar for 30 minutes to obtain powder E. Spread powder E flatly and place it in a porcelain boat in a tube furnace, then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted. Then, heat the tube furnace to 650°C at a heating rate of 7°C / min, and then keep it warm for 4 hours. After the product is cooled, take it out and grind it for 30 minutes to obtain powder F, that is, Ni3ZnC 0.7 @C promoter;

[0076] Step 4: First, mix powder F and powder B in a mass ratio of 1:8, then evacuate the tube furnace to a vacuum state, slowly introduce argon, and repeat the operation three times until all the air in the tube furnace is exhausted, then heat the tube furnace to 350°C at a heating rate of 4°C / min, and then keep it warm for 3h. After the product is cooled, take it out to obtain Ni3ZnC 0.7 @C / g-C3N4 photocatalyst;

[0077] The LabSolar 6A equipment was used to measure the Ni3ZnC 0.7 @C / g-C3N4 was used to test the photocatalytic effect. The specific test process includes weighing 30 mg of the composite photocatalyst and 15 mL of isopropanol, placing them in a glass reaction container filled with 85 mL of deionized water, and irradiating them with light for 4 hours.

[0078] The above specific embodiments are only selected examples to clearly illustrate the effects that can be achieved by the present invention, and cannot be simply considered as all implementation schemes of the present invention. For practitioners in the relevant field, other changes can be made on the basis of the above scheme description, which cannot be exhaustively listed here. Any changes in numerical values ​​derived from the design principles of the present invention still fall within the scope of protection of the claims of the present invention.

Claims

1. A Ni3ZnC 0.7 The preparation method of @C / g-C3N4 photocatalyst is characterized in that: The following steps are involved: Step 1: Prepare nano-sheet g-C3N4 by a one-step calcination method; Step 2, nickel chloride, zinc acetate, urea and acetylacetone are mixed in a molar ratio of (1-3):(1-2):(1-5):(0.1-0.6) to obtain a mixed powder, and then the mixed powder and the nano-sheet g-C3N4 prepared in step 1 are mixed in a mass ratio of 1:(1-6), water and ethylene glycol mixed solution are added, ultrasonic treatment is performed, and then the mixture is stirred until uniformly dispersed, and then poured into the lining of a reactor, placed in a vacuum drying oven at 100-160°C for 10-16h, and the reactor is taken out after the temperature in the oven drops to room temperature, centrifuged, washed, and dried to obtain NiZn-LDH / g-C3N4; Step 3: Mix the NiZn-LDH / g-C3N4 prepared in step 2 with melamine in a mass ratio of (0.5-4):(1-10), grind and spread on a porcelain boat and then place it in a tube furnace. In an argon atmosphere, heat the tube furnace to 500-700°C at a rate of 5-10°C / min, keep warm for 2-4h, and after the product is cooled, take out and grind to obtain Ni3ZnC 0.7 @C promoter; Step 4: First, the Ni3ZnC prepared in step 3 0.7 The @C co-catalyst and the nano-sheet g-C3N4 prepared in step 1 are mixed in a mass ratio of (0.5-1):(5-10) and placed in a tube furnace. The tube furnace is heated to 200-400°C at a rate of 2-5°C / min under an argon atmosphere and kept warm for 1-3h. After the product is cooled, it is taken out to obtain Ni3ZnC 0.7 @C / g-C3N4 photocatalyst.

2. Ni3ZnC as claimed in claim 1 0.7 The preparation method of @C / g-C3N4 photocatalyst is characterized in that: The specific steps of preparing nano-sheet g-C3N4 by the one-step calcination method described in step 1 include: Urea and dicyandiamide are sequentially placed in a beaker containing a sulfuric acid solution in a mass ratio of (1-5):(1-3), and stirred for 1-3 hours. Finally, the mixed solution is placed in a water bath and heated at 60-80°C for 1-6 hours. After the reaction is completed, the cooled reaction solution is poured out, centrifuged, and washed to obtain solid A. The volume ratio of 1M concentrated sulfuric acid to ultrapure water in the sulfuric acid solution is (1-2):(2-5); Spread solid A on a porcelain boat, place it in a tube furnace under air atmosphere, heat it to 450-600°C at a rate of 2-10°C / min, and keep it warm for 1-4h. After calcination, the sample is naturally cooled in the furnace and ground to obtain yellow powder B, i.e., flaky g-C3N4.

3. Ni3ZnC as claimed in claim 1 0.7 The preparation method of @C / g-C3N4 photocatalyst is characterized in that: The volume ratio of ethylene glycol to ultrapure water in the water and ethylene glycol mixture described in step 2 is (1-2):(3-5).

4. Ni3ZnC as claimed in claim 1 0.7 The preparation method of @C / g-C3N4 photocatalyst is characterized in that: The ultrasonic treatment time in step 2 is 30-120 min.

5. Ni3ZnC as claimed in claim 1 0.7 The preparation method of @C / g-C3N4 photocatalyst is characterized in that: The stirring in step 2 is to place the mixture on a magnetic stirrer and stir for 60-150 minutes.

6. Ni3ZnC according to claim 1 or 2 0.7 The preparation method of @C / g-C3N4 photocatalyst is characterized in that: The washing is performed by washing with deionized water and anhydrous ethanol for 3-5 times respectively.

7. Ni3ZnC as claimed in claim 1 0.7 The preparation method of @C / g-C3N4 photocatalyst is characterized in that: The drying in step 2 is carried out in a vacuum drying oven for 10-20 hours.

8. Ni3ZnC according to claim 1 or 2 0.7 The preparation method of @C / g-C3N4 photocatalyst is characterized in that: The grinding is performed by placing the mixture in a mortar and grinding it for 30-120 minutes.

9. Ni3ZnC prepared by the method according to any one of claims 1 to 8 0.7 @C / g-C3N4 photocatalyst.

10. A Ni3ZnC as claimed in claim 9 0.7 Application of @C / g-C3N4 photocatalyst in photocatalytic hydrogen production.

Citation Information

Patent Citations

  • One-dimensional porous nanocomposite and preparation method thereof and application in water electrolysis

    CN108611658A

  • Ni3C@Ni core-shell catalyst promoter and Ni3C@Ni / photocatalyst composite material and preparation methods and applications of Ni3C@Ni core-shell catalyst promoter and Ni3C@Ni / photocatalyst composite material

    CN109174144A

  • Fe3C nano particles with core-shell structure and preparation method and application thereof

    CN109395759A

  • Composite photocatalyst and preparation method thereof

    CN111036269A

  • Ni / VN / g-C3N4 composite photocatalyst as well as preparation method and application thereof

    CN115069291A