Catalyst for preparing methanol through in-situ catalysis of methane as well as preparation method and application of catalyst
By dispersing precious metal nanoparticles on metal organic frame materials, the in-situ synthesis and efficient decomposition of oxidants are solved, and the problems of high cost and low catalytic efficiency of oxidants in partial oxidation of methane to methanol are improved, catalytic activity and selectivity are improved, and industrialization is achieved. Promotional potential.
Patent Information
- Application Number
- CN202411247418.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-06
AI Technical Summary
In the prior art, there are problems such as high oxidant cost, low oxidant utilization efficiency and poor catalyst catalytic efficiency in the process of partial oxidation of methane to methanol.
Through hydrothermal synthesis-liquid phase reduction deposition, noble metal nanoparticles are dispersed onto metal organic frame materials with redox pairs to form a transition metal MOF material in a mixed valence state, realizing in-situ synthesis and efficient decomposition of oxidants, and thus efficiently efficiently Activate methane.
It reduces the reaction cost, improves methane catalytic activity and methanol selectivity, simplifies the catalyst preparation process, and has the potential for industrial application.
Smart Images

Figure CN119056493A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysis, and in particular to a catalyst for in-situ catalytic production of methanol from methane, and a preparation method and application thereof. Background Art
[0002] Methane is the main component of natural gas and a cheap resource with huge reserves. However, its direct combustion as a fuel or its emission into the environment will lead to energy consumption and environmental problems. Therefore, upgrading methane to methanol, a high-value oxygenated compound, is an effective way to achieve a sustainable chemical industry. Hydrogen peroxide, as an environmentally friendly oxidant, can activate methane to produce methanol under mild conditions. However, the industrial price of hydrogen peroxide is more expensive than methanol. Using H2 and O2 to produce hydrogen peroxide in situ to oxidize methane is an effective way. Therefore, designing a high-performance catalyst for coupling the in situ hydrogen peroxide generation and hydrogen peroxide decomposition to activate methane is a hot topic and difficulty in research.
[0003] Precious metals such as Au, Ag, and Pd are considered to be active metals for the in-situ synthesis of hydrogen peroxide from H2 and O2. Smaller metal particle size (1-3 nm) and higher metal particle dispersion are important factors for improving the efficiency of hydrogen peroxide generation (Journal of Catalysis, 2017, 349, 30-40). In addition, transition metal organic framework materials containing mixed valence states can improve the efficiency of hydrogen peroxide decomposition through rapid redox cycles due to the presence of redox pairs (J.Am.Chem.Soc.2018, 140, 12469-12475), thereby efficiently activating methane.
[0004] CN117299199A discloses a catalyst for producing methanol by oxidation of methane, the catalyst comprising a molecular sieve carrier and an active metal element loaded on the molecular sieve carrier, wherein the active metal is Au. The catalyst preparation process is simple, the preparation can be repeated, and the catalyst has high stability and can be used repeatedly. The invention also discloses a method for producing methanol by oxidation of methane, which uses carbon monoxide, oxygen and water to generate hydrogen peroxide in situ, and then reacts with methane to achieve a one-step direct oxidation to produce methanol. Carbon monoxide is easy to obtain and inexpensive, and its explosion limit range is narrower than that of hydrogen, which improves operational safety; and the route of the present invention has excellent methane conversion rate and methanol selectivity, and has certain industrial application prospects.
[0005] Therefore, the focus of reaction research is to highly disperse precious metal nanoparticles on organic framework materials with transition metal redox pairs to prepare catalysts that can efficiently generate and decompose H2O2 and activate methane. Summary of the invention
[0006] The present invention aims at solving the problems of high oxidant cost, low oxidant utilization efficiency and poor catalyst catalytic efficiency in the existing partial oxidation of methane to methanol, and provides a method for preparing a catalyst for in-situ catalytic methane preparation of methanol. The catalyst can in-situ synthesize hydrogen peroxide as an oxidant and quickly decompose hydrogen peroxide, thereby efficiently activating methane and having high catalytic activity.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] A method for preparing a catalyst for in-situ catalytic production of methanol from methane comprises the following steps:
[0009] Step 1, mixing a metal precursor solution with a carbon source or a nitrogen source, and performing a sealed hydrothermal synthesis reaction to obtain a MOF containing at least two valent metals;
[0010] Step 2, adding a reducing agent solution to the noble metal precursor solution to obtain a noble metal nanoparticle solution through a reduction reaction;
[0011] Step 3, dispersing the MOF in step 1 in a noble metal nanoparticle solution, and removing the solvent by drying to obtain the catalyst.
[0012] In the present invention, the noble metal is dispersed and loaded on a metal organic framework with a redox pair by a hydrothermal synthesis-liquid phase reduction deposition method, realizing the in-situ synthesis of the oxidant, the efficient decomposition and the coupling process of methane oxidation, and the mixed valence transition metal is bridged by carbon, nitrogen or oxygen to form a MOF material, and then the noble metal is loaded. The catalyst can synthesize hydrogen peroxide as an oxidant in situ, and then the transition metal redox pair quickly decomposes hydrogen peroxide, thereby efficiently activating methane. The application of the catalyst in the preparation of methanol from methane can not only reduce the reaction cost, but also obtain higher methane catalytic activity and methanol selectivity.
[0013] The metal precursor includes one or a combination of two or more of a halide, nitrate or other complex salt of iron, cobalt or copper;
[0014] The carbon source includes benzoic acid and / or terephthalic acid; the nitrogen source includes one or a combination of two or more of urea, melamine or dicyandiamide; the nitrogen source and the carbon source can form a MOF in which mixed-valence transition metals are bridged by carbon, nitrogen or oxygen.
[0015] The noble metal precursor includes one or a combination of two or more of platinum, gold or silver halides, nitrates or other complex salts; further preferred are hexachloroplatinic acid, potassium chloroplatinate, palladium nitrate, palladium chloride and the like and their hydrates.
[0016] The reducing agent includes one or a combination of two or more of ascorbic acid, sodium borohydride, hydrazine hydrate, sodium citrate, ethylene glycol, and ammonium formate. Sodium borohydride is preferred because it is relatively stable to water and oxygen in the air, easy to handle, and can be promoted and applied to industrial scale.
[0017] In step 1, the hydrothermal synthesis reaction temperature is 140-200°C, and the reaction time is 4-24h. Too high or too low temperature and time will affect the purity and crystallinity of the generated MOF. Preferably, the hydrothermal synthesis reaction temperature is 150-180°C, and the reaction time is 10-20h; further preferably, the hydrothermal synthesis reaction temperature is 170-180°C, and the reaction time is 10-15h;
[0018] The molar ratio of metals in different valence states in the MOF containing at least two valence states is 1:10-10:1. Preferably, the molar ratio of metals in different valence states is 1:2-5:1, and more preferably 1:2-2:1.
[0019] Preferably, MOF contains iron or copper in different valence states, such as Fe 3+ , Fe 2+ , Cu 2+ .
[0020] In step 1, the molar ratio of the metal precursor to the nitrogen source or carbon source is 1:5-5:1.
[0021] The mass ratio of the reducing agent to the noble metal precursor is 1-100:1. If the mass ratio is too low, the noble metal cannot be completely reduced to nanoparticles, and if it is too high, the size of the noble metal particles will increase. The reduction reaction temperature is 0-60°C, preferably 0-40°C, and more preferably 5-30°C. If the reduction temperature is too high, the size of the noble metal particles will increase, which is not conducive to catalytic activity. The time is 5-30 minutes. If the time is too long, the size of the noble metal particles will increase.
[0022] The mass of the noble metal in the noble metal nanoparticle solution in step 3 is 0.5-3wt% of the mass of MOF, preferably 0.5-1wt%. Reducing the noble metal loading is beneficial to reducing the catalyst preparation cost.
[0023] The invention also provides a catalyst prepared by the preparation method.
[0024] The invention also provides application of the catalyst in catalyzing methane to prepare methanol.
[0025] Preferably, in the reaction process for preparing methanol, the reaction temperature is: 25-90°C; the reaction time is: 0.5-2h; the oxygen pressure is: 0.3-0.8MPa; the hydrogen pressure is: 0.8-1.5MPa; the methane pressure is: 1.5-3MPa; and the mass ratio of the catalyst to the methane is: 1:5-1:50.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The present invention disperses and loads precious metals onto a metal-organic framework having a redox pair through a simple hydrothermal synthesis-liquid phase reduction deposition method, thereby achieving the in-situ synthesis of the oxidant, the efficient decomposition and the coupled process of methane oxidation. The catalyst exhibits excellent catalytic performance in the partial oxidation of methane to methanol.
[0028] (2) The present invention couples the two processes of in-situ generation of oxidant and methane oxidation through a simple catalyst preparation process, thereby reducing the reaction cost and facilitating the industrial promotion of the catalyst. In addition, the catalyst preparation process is simple and easy to operate, and the raw materials are simple and easy to obtain, which has the potential for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is Fe in Example 2 3+ -Fe 2+ -MOF materials and prepared Pd / Fe 3+ -Fe 2+ -XRD pattern of MOF catalyst.
[0030] Figure 2 The Pd / Fe prepared in Example 2 3+ -Fe 2+ -TEM image of MOF catalyst.
[0031] Figure 3 The Pd / Fe prepared in Example 2 3+ -Fe 2+ -XPS pattern of Pd in MOF catalyst.
[0032] Figure 4 The Pd / Fe prepared in Example 2 3+ -Fe 2+ -Mössbauer spectrum of Fe in MOF catalyst.
[0033] Figure 5 This is a graph for evaluating the reaction performance of partial oxidation of methane to methanol in Examples 1-4 and Comparative Examples 1-3. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.
[0035] The raw materials used in the following specific embodiments are all purchased from the market.
[0036] Example 1Fe 3+ -Fe 2+ -MOF supported 1wt% Pd catalyst
[0037] (1) Disperse 2 mol of ferric chloride in 20 mL of formamide, then add 2 g of dicyandiamide to the above solution to form a mixed solution, transfer the mixed solution to a hydrothermal reactor, and hydrothermal it at 150°C for 18 h to obtain Fe 3+ -Fe 2+ -MOF material; ferric chloride and dicyandiamide are put into a hydrothermal reactor and react therein, and after crystal nucleation and growth, a Fe bonded with a cyanide group is formed. 2+ and Fe 3+ Mixed MOF structure, there is a redox balance between divalent iron and trivalent iron, maintaining structural stability, and Fe 3+ :Fe 2+ The molar ratio is 4:1.
[0038] (2) 2.5 mg of the noble metal precursor Pd(NO3)2·2H2O was prepared into a 40 mL solution, and a fresh NaBH4 solution was prepared with a mass ratio of the reducing agent NaBH4 to the noble metal precursor of 28:1 and slowly added dropwise thereto at one time, and continued to stir at room temperature for 0.5 h to obtain a solution containing Pd nanoparticles;
[0039] (3) 100 mg Fe 3+ -Fe 2+ -MOF material was added to the above-mentioned Pd nanoparticle solution, with the Pd metal mass being 1wt% of the MOF material, and stirring was continued for 0.5h, and then the solution was dried in a rotary evaporator to obtain Fe 3+ -Fe 2+ -MOF material supported Pd catalyst, denoted as Pd / Fe 3+ -Fe 2+ -MOF.
[0040] Example 2Fe 3+ -Fe 2+ -MOF supported 1wt% Pd catalyst
[0041] (1) Disperse 2 mol of ferric chloride in 20 mL of formamide, then add 2 g of dicyandiamide to the above solution to form a mixed solution, transfer the mixed solution to a hydrothermal reactor, and hydrothermal at 180 ° C for 12 h to obtain Fe 3+ -Fe 2+ -MOF materials; after verification, it is not the theoretical Fe2+ The more the better. Under the experimental conditions currently explored, Fe was obtained by hydrothermal treatment at 180 °C for 12 h. 3 + :Fe 2+ The molar ratio of 1:2 is the best because the Fenton reaction (decomposition of H2O2) requires Fe 3+ , Fe 2+ Participate simultaneously, thus forming a continuous reaction cycle.
[0042] Fe 2+ +H2O2→Fe 3+ +OH - + OH
[0043] Fe 3+ +H2O2→Fe 2+ +H + + OH
[0044] (2) 2.5 mg of the noble metal precursor Pd(NO3)2·2H2O was prepared into a 40 mL solution, and a fresh NaBH4 solution was prepared with a mass ratio of the reducing agent NaBH4 to the noble metal precursor of 28:1 and slowly added dropwise thereto at one time, and continued to stir at room temperature for 0.5 h to obtain a solution containing Pd nanoparticles;
[0045] (3) 100 mg Fe 3+ -Fe 2+ -MOF material was added to the above-mentioned Pd nanoparticle solution, with the Pd metal mass being 1wt% of the MOF material, and stirring was continued for 0.5h, and then the solution was dried in a rotary evaporator to obtain Fe 3+ -Fe 2+ -MOF material supported Pd catalyst, denoted as Pd / Fe 3+ -Fe 2+ -MOF.
[0046] The main difference from Example 1 is the different synthesis temperature and time. At a higher temperature, Fe 2+ The oxidation rate of Fe may increase, and shorter reaction time may lead to 2+ and Fe 3+ The ratio of Fe 2+ Oxidized to Fe 3+ By optimizing the synthesis conditions, Example 2 was selected as the best synthesis condition.
[0047] Figure 1 is Fe in Example 2 3+ -Fe 2+ -MOF materials and prepared Pd / Fe 3+ -Fe2+ -XRD diagram of MOF catalyst. It can be seen that the MOF material was successfully synthesized. In addition, there is no diffraction peak of Pd nanoparticles, indicating that the Pd nanoparticles have a small particle size and high dispersion.
[0048] Figure 2 The Pd / Fe prepared in Example 2 3+ -Fe 2+ -TEM image of MOF catalyst. It can be seen that Pd nanoparticles are effectively supported on the MOF material.
[0049] Figure 3 The Pd / Fe prepared in Example 2 3+ -Fe 2+ -XPS graph of Pd in MOF catalyst. It can be seen that the Pd nanoparticles are 0 valent.
[0050] Figure 4 The Pd / Fe prepared in Example 2 3+ -Fe 2+ -Mössbauer spectrum of Fe in MOF catalyst. It can be seen that Fe 3+ and Fe 2+ The molar ratio is 1:2.
[0051] Example 3Fe 3+ -Cu 2+ -MOF supported 1wt% Pd catalyst
[0052] (1) Disperse 1 mol of ferric chloride and 1 mol of cupric chloride in 20 mL of deionized water, then add 2 g of dicyandiamide to the above solution to form a mixed solution, transfer the mixed solution to a hydrothermal reactor, and hydrothermal the mixture at 180 ° C for 12 h to obtain Fe 3+ -Cu 2+ -MOF material; the actual molar ratio of iron and copper ions in the product is 1:1, which is consistent with the molar ratio of the input raw materials ferric chloride and cupric chloride.
[0053] (2) 2.5 mg of the noble metal precursor Pd(NO3)2·2H2O was prepared into a 40 mL solution, and a fresh NaBH4 solution was prepared with a mass ratio of the reducing agent NaBH4 to the noble metal precursor of 28:1 and slowly added dropwise thereto at one time, and continued to stir at room temperature for 0.5 h to obtain a solution containing Pd nanoparticles;
[0054] (3) 100 mg Fe 3+ -Cu 2+ -MOF material was added to the above-mentioned Pd nanoparticle solution, with the Pd metal mass being 1wt% of the MOF material, and stirring was continued for 0.5h, and then the solution was dried in a rotary evaporator to obtain Fe 3+ -Cu 2+-MOF material supported Pd catalyst, denoted as Pd / Fe 3+ -Cu 2+ -MOF.
[0055] Example 4Fe 3+ -Fe 2+ -MOF supported 1wt% Au catalyst
[0056] (1) Disperse 2 mol of ferric chloride in 20 mL of formamide, then add 2 g of urea to the above solution to form a mixed solution, transfer the mixed solution to a hydrothermal reactor, and hydrothermal it at 180 ° C for 12 h to obtain Fe 3+ -Fe 2+ -MOF materials;
[0057] (2) 1.5 mg of the noble metal precursor AuCl3 was prepared into a 40 mL solution, and a fresh NaBH4 solution was prepared with a mass ratio of the reducing agent NaBH4 to the noble metal precursor of 28:1 and slowly added dropwise thereto at one time, and continued to stir at room temperature for 0.5 h to obtain a solution containing Au nanoparticles;
[0058] (3) 100 mg Fe 3+ -Fe 2+ -MOF material was added to the above Au solution, the Au metal mass was 1wt% of the MOF material, stirring was continued for 0.5h, and then the solution was dried in a rotary evaporator to obtain Fe 3+ -Fe 2+ - Au catalyst supported by MOF material, denoted as Au / Fe 3+ -Fe 2+ -MOF.
[0059] Comparative Example 1 PCN loaded with Fe 3+ catalyst
[0060] (1) Dissolve 3 mg of ferric chloride in water, add 97 mg of PCN polymeric carbon nitride support to the ferric chloride solution, and stir for 0.5 h;
[0061] (2) The above solution was dried in a rotary evaporator, and the obtained solid was ground and calcined in a muffle furnace at 500° C. for 5 h to obtain a Fe2O3 / PCN catalyst.
[0062] Comparative Example 2 PCN-supported Pd catalyst
[0063] (1) 2.5 mg of Pd(NO3)2·2H2O as a noble metal precursor was prepared into a 40 mL solution, and a fresh NaBH4 solution was prepared according to a mass ratio of reducing agent NaBH4 to noble metal precursor of 28:1 and slowly added dropwise thereto at one time, and continued stirring at room temperature for 0.5 h to obtain a solution containing Pd nanoparticles;
[0064] (2) 100 mg of PCN carrier was added to the above Pd solution and stirred for 0.5 h. The mass of Pd metal was 1 wt% of the PCN material. The solution was then dried in a rotary evaporator to obtain a Pd catalyst supported by PCN material, which was recorded as Pd / PCN.
[0065] Comparative Example 3Fe 3+ -MOF supported 1wt% Pd catalyst
[0066] (1) 2 mol of ferric chloride was dispersed in 20 mL of deionized water, and then 2 g of terephthalic acid was added to the above solution to form a mixed solution. The mixed solution was transferred to a hydrothermal reactor and hydrothermalized at 150 ° C for 18 h to obtain Fe 3+ -MOF materials;
[0067] (2) 2.5 mg of the noble metal precursor Pd(NO3)2·2H2O was prepared into a 40 mL solution, and a fresh NaBH4 solution was prepared with a mass ratio of the reducing agent NaBH4 to the noble metal precursor of 28:1 and slowly added dropwise thereto at one time, and continued to stir at room temperature for 0.5 h to obtain a solution containing Pd nanoparticles;
[0068] (3) 100 mg Fe 3+ -MOF material was added to the above-mentioned Pd nanoparticle solution, with the Pd metal mass being 1wt% of the MOF material, and stirring was continued for 0.5h, and then the solution was dried in a rotary evaporator to obtain Fe 3+ -MOF material supported Pd catalyst, denoted as Pd / Fe 3+ -MOF.
[0069] Catalyst performance evaluation
[0070] The performance of the catalysts prepared in the examples and comparative examples in the partial oxidation of methane to methanol was evaluated, and the reaction was carried out in an autoclave reactor.
[0071] Application Example 1
[0072] Step 1, weigh 10 mg of the catalyst of Examples 1-4 and Comparative Examples 1-3, fill it into the quartz liner of a kettle reactor, then add 40 mL of water into the liner, and tighten the kettle reactor;
[0073] Step 2, then introduce O2 to replace the air in the reactor, introduce 0.3MPa-O2, 0.8MPa-H2 and 1.5MPa-CH4, set the reaction temperature to 50°C, and the reaction time to 0.5h.
[0074] Step 3: After the reaction is completed, the reactor is placed in an ice-water bath. After the reaction temperature drops to room temperature, the liquid after the reaction is centrifuged, the supernatant is taken for liquid nuclear magnetic resonance analysis, and the product yield and methanol selectivity are calculated by the external standard method. Figure 5 The data are comparative data of the reaction performance of partial oxidation of methane to methanol between Examples 1-4 and Comparative Examples 1-3.
[0075] Table 1 Performance evaluation results of catalytic partial oxidation of methane to methanol in Examples 1-4 and Comparative Examples 1-3
[0076]
[0077] from Figure 5 As shown in Table 1, Fe 3+ and Fe 2+ The performance is optimal when the molar ratio is 1:2. The reason why the performance of Example 2 is improved compared with Example 1 is that the optimal Fe 3+ and Fe 2+ Molar ratio, Fe 3+ and Fe 2+ The redox pairs between them are constantly circulating, which improves the efficiency of decomposing H2O2 into OH, thereby improving the activation of methane and promoting the production of methanol. Example 3 Performance is average because the coupling between Fe and other metals is not as good as Fe 3+ and Fe 2+ The redox efficiency of H2O2 is high. The performance of Example 4 is average because Au, as an active metal for in-situ synthesis of H2O2 by H2 and O2, is not as high as the yield of H2O2 synthesized by Pd. But overall, it is far better than Comparative Examples 1-3.
Claims
1. A method for preparing a catalyst for in-situ catalytic production of methanol from methane, characterized in that: Includes steps: Step 1, mixing a metal precursor solution with a carbon source or a nitrogen source, and performing a sealed hydrothermal synthesis reaction to obtain a MOF containing at least two valent metals; Step 2, adding a reducing agent solution to the noble metal precursor solution to obtain a noble metal nanoparticle solution through a reduction reaction; Step 3, dispersing the MOF in step 1 in a noble metal nanoparticle solution, and removing the solvent by drying to obtain the catalyst.
2. The method for preparing a catalyst for in-situ catalytic production of methanol from methane according to claim 1, characterized in that: The metal precursor includes one or a combination of two or more of a halide, nitrate or other complex salt of iron, cobalt or copper; and / or, the carbon source comprises benzoic acid and / or terephthalic acid; And / or, the nitrogen source comprises one or a combination of two or more of urea, melamine or dicyandiamide; And / or, the noble metal precursor includes one or a combination of two or more of platinum, gold or silver halides, nitrates or other complex salts; And / or, the reducing agent includes one or a combination of two or more of ascorbic acid, sodium borohydride, hydrazine hydrate, sodium citrate, ethylene glycol, and ammonium formate.
3. The method for preparing a catalyst for in-situ catalytic production of methanol from methane according to claim 1, characterized in that: In step 1, the hydrothermal synthesis reaction temperature is 140-200° C., and the reaction time is 4-24 hours.
4. The method for preparing a catalyst for in-situ catalytic production of methanol from methane according to claim 1, characterized in that: The molar ratio of metals with different valence states in the MOF containing at least two valence state metals is 1:10-10:
1.
5. The method for preparing a catalyst for in-situ catalytic production of methanol from methane according to claim 1, characterized in that: In step 1, the molar ratio of the metal precursor to the nitrogen source or carbon source is 1:5-5:
1.
6. The method for preparing a catalyst for in-situ catalytic production of methanol from methane according to claim 1, characterized in that: The mass ratio of the reducing agent to the noble metal precursor is 1-100:1; the reduction reaction temperature is 0-60° C., and the time is 5-30 min.
7. The method for preparing a catalyst for in-situ catalytic production of methanol from methane according to claim 1, characterized in that: In step 3, the mass of the noble metal in the noble metal nanoparticle solution is 0.5-3 wt % of the mass of the MOF.
8. A catalyst prepared according to the preparation method according to any one of claims 1 to 7.
9. Use of the catalyst according to claim 8 in catalyzing the production of methanol from methane.
10. The use according to claim 9, characterized in that: In the reaction process of preparing methanol, the reaction temperature is: 25-90°C; the reaction time is: 0.5-2h; the oxygen pressure is: 0.3-0.8MPa; the hydrogen pressure is: 0.8-1.5MPa; the methane pressure is: 1.5-3MPa; the mass ratio of the catalyst to the methane is: 1:5-1:50.
Citation Information
Patent Citations
Preparation method of metal organic framework for loading nano silver
CN106582857A
Water-stable mixed-valence MOF (Metal Organic Framework) material, preparation method thereof and application of water-stable mixed-valence MOF material in photocatalytic water decomposition
CN114989447A
Preparation method and application of bimetallic MOF anchored Pt nanocluster catalyst
CN115770621A
Cited By
Bifunctional modified MOF (Metal Organic Framework) packaged metal catalyst as well as preparation method and application thereof
CN120920077A