Battery aluminum foil coating device and coating method, current collector and battery

By designing the battery aluminum foil coating device, using double-sided coating components and step-by-step coating technology, the problem of large space occupation and high material requirements in the existing technology is solved, and efficient and low-cost battery aluminum foil coating is achieved, which improves the Productivity and flexibility in material selection.

CN119056684APending Publication Date: 2024-12-03QUJING EVE ENERGY CO LTD

Patent Information

Application Number
CN202411186900.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing double-sided coating method of battery aluminum foil requires two equipment to process the first and second sides of aluminum foil respectively, which takes up a large space and high material requirements, which limits the use conditions.

Method used

A battery aluminum foil coating device is designed, including an unwinding mechanism, a double-sided coating assembly, a first-sided coating assembly and a second-sided coating assembly, and the carbon is uniformly applied on both sides of the aluminum foil by the double-sided coating assembly. The layer is coated on the dried carbon coating layer, and the carbon coating layer and electrode layer materials of different systems are allowed to be coated separately.

Benefits of technology

It reduces production costs, shortens production cycles, reduces resource waste, saves equipment space, and reduces material compatibility requirements, improving coating efficiency and accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056684A_ABST
    Figure CN119056684A_ABST
Patent Text Reader

Abstract

The invention discloses a battery aluminum foil coating device, a coating method, a current collector and a battery, an aluminum foil sequentially passes through an unwinding mechanism, a double-sided coating assembly, a first surface coating assembly, a second surface coating assembly and a winding mechanism to finish double-sided coating, so that an aluminum foil carbon layer coating process and an electrode slurry coating process are combined; the production cost is greatly reduced, the production period is shortened, and the resource waste is reduced; moreover, compared with the prior art in which two sets of equipment are needed for coating the first surface and the second surface of the aluminum foil with the carbon layer coating slurry respectively, the coating function is integrated through the design of the double-surface coating assembly, and the occupied space of the coating device is greatly saved; meanwhile, the two faces of the aluminum foil can be coated with carbon coating layers through the double-face coating assembly respectively, the carbon coating layers are coated with electrode layers through the first face coating assembly and the second face coating assembly respectively, carbon coating layer slurry and electrode slurry of different systems are allowed to be used through the step-by-step coating technology, and the requirement for material compatibility is lowered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a battery aluminum foil coating device and coating method, a current collector and a battery. Background Art

[0002] At present, the use of functional coatings to treat the surface of battery conductive substrates is a breakthrough technological innovation. Carbon-coated aluminum foil or copper foil is to evenly and finely coat the dispersed nano-conductive graphite and carbon-coated particles on aluminum foil or copper foil. It can provide excellent static conductivity, collect the microcurrent of active substances, improve the processing performance of the positive and negative electrodes of the battery, and enhance battery performance.

[0003] In the relevant design, the battery aluminum foil is processed by a double-sided coating method. First, the carbon coating slurry and the electrode slurry are mixed, and then the coating is completed on the front and back of the aluminum foil respectively. Although this method can save resources and reduce operating costs, it requires two coating equipment and occupies a large space. In addition, this method requires the use of the same system of carbon coating slurry and electrode slurry, which has high requirements on materials and limits its use conditions. Summary of the invention

[0004] The embodiments of the present application provide a battery aluminum foil coating device and coating method, a current collector and a battery, which are used to solve or at least partially solve the deficiencies of the above-mentioned background technology.

[0005] In a first aspect, an embodiment of the present application provides a battery aluminum foil coating device, comprising:

[0006] Unwinding mechanism, used for unwinding aluminum foil;

[0007] A double-sided coating assembly is used to first coat the carbon coating slurry on the first side of the aluminum foil, then coat the carbon coating slurry on the second side of the aluminum foil, and finally dry the coated first side and second side of the aluminum foil simultaneously;

[0008] A first-side coating assembly is used to sequentially coat the electrode slurry and the ceramic insulating slurry on the first side of the aluminum foil, and dry the coated first side of the aluminum foil;

[0009] A second side coating assembly is used to sequentially coat the electrode slurry and the ceramic insulating slurry on the second side of the aluminum foil, and dry the coated second side of the aluminum foil;

[0010] The winding mechanism is used to wind up the coated aluminum foil;

[0011] The aluminum foil passes through the unwinding mechanism, the double-sided coating assembly, the first-sided coating assembly, the second-sided coating assembly and the winding mechanism in sequence to complete double-sided coating.

[0012] In one embodiment, the double-sided coating assembly is located between the unwinding mechanism and the first-sided coating assembly, and the double-sided coating assembly includes a double-sided carbon layer coating mechanism and a drying mechanism connected in sequence;

[0013] The first-side coating assembly is located between the double-side coating assembly and the second-side coating assembly, the first-side coating assembly includes a first-side coating mechanism and a first oven connected in sequence, and the second-side coating assembly includes a second-side coating mechanism and a second oven connected in sequence.

[0014] In one embodiment, the double-sided carbon layer coating mechanism comprises:

[0015] Frame;

[0016] A first carbon layer coating mechanism, used for coating a carbon layer coating slurry on a first surface of the aluminum foil;

[0017] A second carbon layer coating mechanism, used for coating a carbon layer slurry on the second surface of the aluminum foil;

[0018] Wherein, the first carbon layer coating mechanism and the second carbon layer coating mechanism are both located in the frame, and the aluminum foil passes through the first carbon layer coating mechanism and the second carbon layer coating mechanism in sequence.

[0019] In one embodiment, the battery aluminum foil coating device further includes a deviation correction mechanism, and the deviation correction mechanism is arranged between the unwinding mechanism and the double-sided coating assembly;

[0020] And / or, the deviation correcting mechanism is arranged between the drying mechanism and the first-side coating mechanism;

[0021] And / or, the deviation correction mechanism is arranged between the first oven and the second surface coating mechanism;

[0022] And / or, the deviation correcting mechanism is arranged between the second oven and the winding mechanism.

[0023] In a second aspect, an embodiment of the present application provides a method for coating a battery aluminum foil, the method for coating a battery aluminum foil comprising at least the following steps:

[0024] After the aluminum foil roll is unrolled by the unwinding mechanism, the aluminum foil is fed into the double-sided coating assembly;

[0025] The aluminum foil enters the double-sided coating assembly, and the double-sided coating assembly first coats the carbon coating slurry on the first side of the aluminum foil, and then coats the carbon coating slurry on the second side of the aluminum foil, and then dries the first side and the second side of the coated aluminum foil at the same time, and finally sends the aluminum foil with the carbon coating to the first side coating assembly;

[0026] The aluminum foil enters the first-side coating assembly, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the first side of the aluminum foil after the carbon coating is completed by the first-side coating assembly, and the first side of the aluminum foil coated with the electrode slurry is dried, and then the aluminum foil is sent to the second-side coating assembly;

[0027] The aluminum foil enters the second side coating assembly, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the second side of the aluminum foil after the carbon coating is completed by the second side coating assembly, and the second side of the aluminum foil coated with the electrode slurry is dried, and then the aluminum foil is sent to the winding mechanism;

[0028] The aluminum foil is rolled up by a rolling mechanism to complete the coating of the aluminum foil.

[0029] In one embodiment, the aluminum foil enters a double-sided coating assembly, and the double-sided coating assembly is used to first coat the carbon coating slurry on the first side of the aluminum foil, and then coats the carbon coating slurry on the second side of the aluminum foil, and then the first side and the second side of the coated aluminum foil are dried simultaneously, and finally the aluminum foil is introduced into the first side coating assembly through a guide roller. The steps include:

[0030] The aluminum foil enters the first carbon layer coating mechanism, the first carbon layer coating mechanism is used to coat the carbon layer coating slurry on the first surface of the aluminum foil, and then the aluminum foil is sent to the second carbon layer coating mechanism;

[0031] The aluminum foil enters the second carbon layer coating mechanism, the second carbon layer coating mechanism is used to coat the carbon layer slurry on the second surface of the aluminum foil, and then the aluminum foil is sent to the drying mechanism;

[0032] The aluminum foil enters the drying mechanism, and the first side and the second side of the coated aluminum foil are dried simultaneously by the drying mechanism, and then the aluminum foil coated with the carbon layer is sent to the first side coating assembly.

[0033] In one embodiment, the aluminum foil enters the first-side coating assembly, and the first-side coating assembly is used to sequentially coat the first side of the aluminum foil after the carbon coating is completed with the electrode slurry and the ceramic insulating slurry, and the first side of the aluminum foil after the electrode slurry is coated is dried, and then the aluminum foil is fed into the second-side coating assembly. The steps include:

[0034] The aluminum foil enters the first side coating mechanism, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the first side of the aluminum foil after the carbon coating is completed by the first side coating mechanism, and then the aluminum foil is sent to the first oven;

[0035] The aluminum foil enters the first oven, the first oven is used to dry the first side of the coated aluminum foil, and then the aluminum foil is sent to the second side coating assembly.

[0036] In one embodiment, the aluminum foil enters the second-side coating assembly, and the second-side coating assembly is used to sequentially coat the second side of the aluminum foil after the carbon coating is completed with the electrode slurry and the ceramic insulating slurry, and the second side of the aluminum foil after the electrode slurry is coated is dried, and then the aluminum foil is sent to the winding mechanism. The steps include:

[0037] The aluminum foil enters the second side coating mechanism, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the second side of the aluminum foil after the carbon coating is completed by the second side coating mechanism, and then the aluminum foil is sent to the second oven;

[0038] The aluminum foil enters the second oven, the second side of the coated aluminum foil is dried by the second oven, and then the aluminum foil is sent to the winding mechanism.

[0039] In one embodiment, the drying temperature of the drying mechanism is in a range of greater than or equal to 70 degrees Celsius and less than or equal to 170 degrees Celsius, and the drying time of the drying mechanism is in a range of greater than or equal to 3 seconds and less than or equal to 9 seconds;

[0040] The drying temperature of the first oven is in the range of greater than or equal to 85 degrees Celsius and less than or equal to 105 degrees Celsius, and the drying time of the aluminum foil in the first oven is in the range of greater than or equal to 2 minutes and less than or equal to 4 minutes;

[0041] The drying temperature of the second oven is in the range of greater than or equal to 90 degrees Celsius and less than or equal to 115 degrees Celsius, and the drying time of the aluminum foil in the second oven is in the range of greater than or equal to 2 minutes and less than or equal to 4 minutes.

[0042] In one embodiment, the solvent system of the carbon coating slurry is different from the solvent system of the electrode slurry.

[0043] In a third aspect, an embodiment of the present application provides a current collector, comprising an aluminum foil, wherein the aluminum foil is manufactured using the above-mentioned battery aluminum foil coating method.

[0044] In a fourth aspect, an embodiment of the present application provides a battery, comprising a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material, and the negative electrode sheet comprises a negative electrode current collector;

[0045] Wherein, at least one of the positive electrode current collector and the negative electrode current collector is the above-mentioned current collector.

[0046] Beneficial effects of the embodiments of the present application: The embodiments of the present application provide a battery aluminum foil coating device and coating method, a current collector and a battery, wherein the double-sided coating is completed by sequentially passing the aluminum foil through the unwinding mechanism, the double-sided coating assembly, the first-side coating assembly, the second-side coating assembly and the winding mechanism, thereby combining the aluminum foil carbon layer coating process and the electrode slurry coating process, thereby greatly reducing the production cost, shortening the production cycle and reducing resource waste; and, compared with the traditional method that requires two devices to respectively coat the first and second sides of the aluminum foil, the present application integrates the coating functions through the design of a double-sided coating assembly, thereby greatly saving the floor space of the coating device; at the same time, the double-sided coating assembly can coat the carbon coating layer on both sides of the aluminum foil, and the first-side coating assembly and the second-side coating assembly can respectively coat the electrode layer on the carbon coating layer, and the step-by-step coating technology allows the use of carbon coating slurries and electrode slurries of different systems, thereby reducing the strict requirements on material compatibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solution in this embodiment, the drawings required for use in the description of the embodiment will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0048] Figure 1 It is a structural schematic diagram of a battery aluminum foil carbon layer coating device in the related art;

[0049] Figure 2 It is a structural schematic diagram of a battery aluminum foil electrode slurry coating device in the related art;

[0050] Figure 3 It is a structural schematic diagram of a battery aluminum foil carbon layer double-sided coating device in the related art;

[0051] Figure 4 A schematic diagram of the structure of a battery aluminum foil coating device provided in an embodiment of the present application;

[0052] Figure 5 A flow chart of a coating method for battery aluminum foil provided in an embodiment of the present application;

[0053] Figure 6 A top view of the first side of the battery aluminum foil provided in the embodiment of the present application after the double-sided coating process is completed;

[0054] Figure 7 A schematic diagram of the structure of the coating main layer provided in an embodiment of the present application;

[0055] Figure 8 A schematic diagram of the structure of the current collector provided in an embodiment of the present application;

[0056] Fig. 9 A schematic diagram of the structure of a battery provided in an embodiment of the present application.

[0057] Description of Reference Numerals

[0058] 1-battery aluminum foil carbon layer coating device; 2-battery aluminum foil electrode slurry coating device; 3-double-sided coating device; 4-battery aluminum foil coating device; 5-current collector; 6-battery;

[0059] 11-first aluminum foil unwinding mechanism; 12-aluminum foil corona mechanism; 13-aluminum foil first side carbon layer coating mechanism; 14-first aluminum foil oven; 15-aluminum foil second side carbon layer coating mechanism; 16-second aluminum foil oven; 17-first aluminum foil winding mechanism;

[0060] 21-second aluminum foil unwinding mechanism; 22-aluminum foil first side electrode slurry coating mechanism; 23-third aluminum foil oven; 24-aluminum foil second side electrode slurry coating mechanism; 25-fourth aluminum foil oven; 26-second aluminum foil rewinding mechanism;

[0061] 31-unwinding mechanism; 32-first side coating assembly; 33-second side coating assembly; 34-rewinding mechanism;

[0062] 41-unwinding mechanism; 42-double-sided coating assembly; 43-first-side coating assembly; 44-second-side coating assembly; 45-winding mechanism; 46-corona mechanism; 47-correction mechanism;

[0063] 421-double-sided carbon layer coating mechanism; 4211-first carbon layer coating mechanism; 4212-second carbon layer coating mechanism; 4213-frame; 422-drying mechanism; 431-first side coating mechanism; 432-first oven; 441-second side coating mechanism; 442-second oven; 471-first deviation correction structure; 473-third deviation correction structure;

[0064] 51-coating layer; 511-coating main layer; 512-ceramic insulating layer; 5111-carbon coating layer; 5112-electrode layer; 52-foil portion; 53-metal layer;

[0065] 61 - positive electrode; 62 - negative electrode; 63 - separator. DETAILED DESCRIPTION

[0066] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0067] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0068] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0069] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0070] This embodiment provides a battery aluminum foil coating device and coating method, a current collector and a battery. The following are detailed descriptions. It should be noted that the description order of the following embodiments is not intended to limit the preferred order of the embodiments.

[0071] See also Figure 4 , is a schematic diagram of the structure of the battery aluminum foil coating device provided in an embodiment of the present application.

[0072] In one embodiment, the battery aluminum foil coating device 4 includes an unwinding mechanism 41, a double-sided coating component 42, a first-side coating component 43, a second-side coating component 44 and a winding mechanism 45. The unwinding mechanism 41 is used to unwind the aluminum foil. The double-sided coating component 42 is used to first coat the carbon coating slurry on the first side of the aluminum foil, then coat the carbon coating slurry on the second side of the aluminum foil, and finally dry the first side and the second side of the coated aluminum foil at the same time. The first-side coating component 43 is used to coat the first side of the aluminum foil according to the first side of the aluminum foil. The electrode slurry and the ceramic insulating slurry are coated on the first side of the aluminum foil in turn, and the coated first side of the aluminum foil is dried. The second side coating assembly 44 is used to sequentially coat the electrode slurry and the ceramic insulating slurry on the second side of the aluminum foil, and dry the coated second side of the aluminum foil. The winding mechanism 45 is used to wind up the coated aluminum foil. The aluminum foil passes through the unwinding mechanism 41, the double-sided coating assembly 42, the first side coating assembly 43, the second side coating assembly 44 and the winding mechanism 45 in turn to complete double-sided coating.

[0073] It can be understood that in this embodiment, the battery aluminum foil coating device 4 includes a unwinding mechanism 41, a double-sided coating component 42, a first-side coating component 43, a second-side coating component 44 and a winding mechanism 45, thereby avoiding interference between different coating processes and improving the overall performance and production efficiency of the equipment; at the same time, the double-sided coating component 42, the first-side coating component 43 and the second-side coating component 44 independently perform specific coating and drying processes, and the parameters of each part can be adjusted according to different needs to adapt to different production conditions and materials.

[0074] In one embodiment, the double-sided coating component 42 is located between the unwinding mechanism 41 and the first-sided coating component 43, and the double-sided coating component 42 includes a double-sided carbon layer coating mechanism 421 and a drying mechanism 422 connected in sequence; the first-side coating component 43 is located between the double-sided coating component 42 and the second-side coating component 44, and the first-side coating component 43 includes a first-side coating mechanism 431 and a first oven 432 connected in sequence; the second-side coating component 44 is located between the first-side coating component 43 and the winding mechanism 45, and the second-side coating component 44 includes a second-side coating mechanism 441 and a second oven 442 connected in sequence; the aluminum foil is double-sided coated by passing through the unwinding mechanism, the double-sided carbon layer coating mechanism 421, the drying mechanism 422, the first-side coating mechanism 431, the first oven 432, the second-side coating mechanism 441, the second oven 442 and the winding mechanism 45 in sequence.

[0075] Furthermore, the double-sided carbon layer coating mechanism 421 is used to first coat the carbon layer coating slurry on the first side of the aluminum foil and then coat the carbon layer coating slurry on the second side of the aluminum foil. The double-sided carbon layer coating mechanism 421 can be located at any position of the front end, rear end, top or bottom of the unwinding mechanism 41, as long as the aluminum foil can be fed into the unwinding mechanism 41, the double-sided carbon layer coating mechanism 421 and the drying mechanism 422 in sequence.

[0076] Specifically, the double-sided carbon layer coating mechanism 421 includes a first carbon layer coating mechanism 4211 and a second carbon layer coating mechanism 4212 which are connected in sequence, the first carbon layer coating mechanism 4211 is used to coat the carbon layer coating slurry on the first side of the aluminum foil, and the second carbon layer coating mechanism 4212 is used to coat the carbon layer coating slurry on the second side of the aluminum foil, and the aluminum foil passes through the first carbon layer coating mechanism 4211 and the second carbon layer coating mechanism 4212 in sequence, thereby ensuring that the aluminum foil can be evenly coated with the carbon layer coating slurry on both sides through the double-sided carbon layer coating mechanism 421, thereby shortening the production cycle; at the same time, by setting the first carbon layer coating mechanism 4211 and the second carbon layer coating mechanism 4212 to process the two sides (the first side and the second side) of the aluminum foil respectively, the coating process parameters (such as coating speed, coating thickness, pressure, etc.) of each side can be independently adjusted to ensure the uniformity and accuracy of the coating.

[0077] In one embodiment, the double-sided carbon layer coating mechanism 421 also includes a frame 4213, and the first carbon layer coating mechanism 4211 and the second carbon layer coating mechanism 4212 are both located in the frame 4213, and the second carbon layer coating mechanism 4212 can be located at any position of the front end, rear end, top or bottom of the first carbon layer coating mechanism 4211, as long as the aluminum foil can be fed into the first carbon layer coating mechanism 4211 and the second carbon layer coating mechanism 4212 in sequence; wherein, this embodiment takes the first carbon layer coating mechanism 4211 and the second carbon layer coating mechanism 4212 being arranged up and down in the frame 4213 as an example to illustrate the technical solution of the present application.

[0078] It can be understood that, in this embodiment, by locating both the first carbon layer coating mechanism 4211 and the second carbon layer coating mechanism 4212 in the frame 4213, the floor space occupied by the equipment and the complexity of the layout are reduced, thereby optimizing the space utilization.

[0079] The drying mechanism 422 is located between the double-sided carbon layer coating mechanism 421 and the first electrode slurry mechanism, and is used to simultaneously dry the first side and the second side of the coated aluminum foil, wherein the heat source of the drying mechanism 422 may be at least one of steam, electric heater, infrared, and microwave, and a suitable drying method may be selected according to actual needs to ensure that the coated aluminum foil can be efficiently dried.

[0080] It should be noted that, in this embodiment, the drying mechanism 422 is an infrared oven as an example to illustrate the technical solution of the present application. The infrared oven adopts infrared radiation heating. The infrared radiation can penetrate the air layer and directly heat the surface of the material, which can quickly increase the temperature and accelerate the drying speed. The drying mechanism 422 may include an oven and a plurality of infrared heating elements located in the oven. The plurality of infrared heating elements are respectively installed at the top and the bottom of the oven. The aluminum foil can be moved inside the oven through a conveyor belt. The design of the conveyor belt can ensure that the aluminum foil moves smoothly under the infrared heating element to ensure that the first side and the second side of the aluminum foil can receive infrared radiation at the same time. At the same time, by adjusting the radiation intensity of the infrared heating elements at the top and the bottom, the uniformity of heating the first side and the second side of the aluminum foil can be controlled.

[0081] In one embodiment, the first-side coating assembly 43 includes a first-side coating mechanism 431 and a first oven 432 which are connected in sequence; wherein the first-side coating mechanism 431 is used to sequentially coat the electrode slurry and the ceramic insulating slurry on the first side of the aluminum foil, and the first oven 432 is used to dry the first side of the aluminum foil after coating.

[0082] It should be noted that, since the first-side coating mechanism 431 sequentially coats the electrode slurry and the ceramic insulating slurry on the dried carbon coating layer, there is no direct contact between the carbon coating layer slurry and the electrode slurry, thereby avoiding chemical reactions and incompatibility problems between them.

[0083] Specifically, the first-side coating mechanism 431 can be located at any position of the front end, rear end, top or bottom of the drying mechanism 422, as long as the aluminum foil can be fed into the first-side coating mechanism 431 and the first oven 432 in sequence; specifically, this embodiment takes the example of the first-side coating mechanism 431 being located between the drying mechanism 422 and the first oven 432 to illustrate the technical solution of the present application.

[0084] The first-side coating mechanism 431 includes a first die head, which can be divided into two areas, one area for full-surface coating of electrode slurry, and the other area for edge coating of ceramic insulating slurry; wherein the two areas can be separated by a fluid isolation structure to ensure that the two materials will not mix in the die head.

[0085] It can be understood that in this embodiment, the first-side coating assembly 43 is provided to include a first-side coating mechanism 431 and a first oven 432 connected in sequence, so that the first-side coating mechanism 431 and the first oven 432 are integrated into a production line, thereby saving space and reducing the footprint of the equipment; at the same time, after the first side and the second side of the aluminum foil are dried by the drying mechanism 422, the first side of the aluminum foil can be immediately coated with electrode slurry by the first-side coating mechanism 431, and then coated with ceramic insulating slurry, and then enter the first oven 432 for drying, thereby reducing the transfer time and operation complexity of the aluminum foil between each step, and simplifying the entire production process; and, avoiding the aluminum foil after the carbon layer is coated from being exposed to the air for a long time, which may cause oxidation and affect the adhesion of the subsequent coating layer.

[0086] It should be noted that the carbon coating slurry forms a uniform coating on the surface of the aluminum foil, so that the microscopic bumps on the surface of the aluminum foil are filled, thereby providing a smoother and more consistent base. That is, in this embodiment, after applying the carbon coating slurry, the electrode slurry is applied, which can ensure the uniformity and adhesion of each layer of the coating; and the carbon coating slurry provides a good conductive foundation, and the coating of the electrode slurry can further improve the performance of the battery.

[0087] In one embodiment, the second-side coating assembly 44 includes a second-side coating mechanism 441 and a second oven 442 which are connected in sequence; wherein the second-side coating mechanism 441 is used to sequentially coat the electrode slurry and the ceramic insulating slurry on the second side of the aluminum foil, and the second oven 442 is used to dry the second side of the aluminum foil after coating.

[0088] Specifically, the second electrode slurry coater can be located at any position of the front end, rear end, top or bottom of the first oven 432, as long as the aluminum foil can be fed into the second-side coating mechanism 441 and the second oven 442 in sequence; specifically, this embodiment takes the example of the second-side coating mechanism 441 being located between the first oven 432 and the second oven 442 to illustrate the technical solution of the present application.

[0089] The second-side coating mechanism 441 includes a second die head, which can be divided into two areas, one area for full-surface coating of electrode slurry, and the other area for edge coating of ceramic insulating slurry; wherein the two areas can be separated by a fluid isolation structure to ensure that the two materials will not mix in the die head.

[0090] It can be understood that in this embodiment, the second-side coating assembly 44 is provided to include a second-side coating mechanism 441 and a second oven 442 connected in sequence, thereby integrating the first-side coating mechanism 431 and the first oven 432 on a production line, saving space and reducing the footprint of the equipment; at the same time, the electrode slurry is coated on the second side of the aluminum foil by the second-side coating mechanism 441, and the second oven 442 dries the second side of the coated aluminum foil, which can ensure that the coatings on both sides (the first side and the second side) of the aluminum foil are processed under the same conditions, thereby ensuring that the thickness and quality of the double-sided coatings are consistent; and, after the first side of the aluminum foil is dried by the first oven 432, the second side of the aluminum foil can be immediately coated with the electrode slurry by the second-side coating mechanism 441, and then enters the second oven 442 for drying.

[0091] It should be noted that carbon-coated aluminum foil or copper foil is to evenly and finely coat the dispersed nano-conductive graphite and carbon-coated particles on the aluminum foil or copper foil. It can provide excellent static conductivity and collect the microcurrent of active substances. It can improve the processing performance of the positive and negative electrodes of the battery and enhance the battery performance. At present, most lithium battery companies directly purchase carbon-coated aluminum foil for coating, which is costly. In order to reduce the cost of incoming materials, some companies purchase lower-priced double-sided smooth aluminum foil, and then perform carbon layer coating and electrode slurry processes on the surface of the aluminum foil in turn, thereby preparing the electrode plates to be cut.

[0092] Specifically, see Figure 1 , which is a structural schematic diagram of a battery aluminum foil carbon layer coating device in the related art; in the related art, the battery aluminum foil carbon layer coating device 1 includes a first aluminum foil unwinding mechanism 11, an aluminum foil corona mechanism 12, an aluminum foil first side carbon layer coating mechanism 13, a first aluminum foil oven 14, an aluminum foil second side carbon layer coating mechanism 15, a second aluminum foil oven 16 and a first aluminum foil winding mechanism 17, wherein the aluminum foil is sequentially fed into the first aluminum foil unwinding mechanism 11, the aluminum foil corona mechanism 12, the aluminum foil first side carbon layer coating mechanism 13, the first aluminum foil oven 14, the aluminum foil second side carbon layer coating mechanism 15, the second aluminum foil oven 16 and the first aluminum foil winding mechanism 17, thereby completing the carbon layer coating process on both sides of the aluminum foil.

[0093] See also Figure 2, which is a structural schematic diagram of a battery aluminum foil electrode slurry coating device in the related art; in the related art, the battery aluminum foil electrode slurry coating device 2 includes a second aluminum foil unwinding mechanism 21, an aluminum foil first side electrode slurry coating mechanism 22, a third aluminum foil oven 23, an aluminum foil second side electrode slurry coating mechanism 24, a fourth aluminum foil oven 25 and a second aluminum foil winding mechanism 26; wherein, the aluminum foil that has completed the double-sided carbon layer coating process is sequentially fed into the second aluminum foil unwinding mechanism 21, the aluminum foil first side electrode slurry coating mechanism, the third aluminum foil oven 23, the aluminum foil second side electrode slurry coating mechanism 24, the fourth aluminum foil oven 25 and the second aluminum foil winding mechanism 26, thereby completing the electrode slurry coating process on both sides of the aluminum foil.

[0094] Combination Figure 1 and Figure 2 It can be seen that in the related technology, the carbon layer coating of aluminum foil and the electrode slurry coating are two discontinuous processes. The aluminum foil carbon coating process and the electrode slurry coating process need to go through two winding and unwinding processes, and the operation is cumbersome. In order to reduce the cost of incoming materials, some companies purchase double-sided smooth aluminum foil with lower prices, and need to add a factory to carry out the carbon coating process on the surface of the aluminum foil. At the same time, the carbon-coated aluminum foil needs to be dried in an oven. After carbon coating, the aluminum foil is sent to the electrode coating workshop for electrode slurry coating. The product realization cycle is long and labor costs are consumed.

[0095] It can be understood that compared with the disadvantage of higher costs caused by directly purchasing carbon-coated aluminum foil for electrode slurry coating, this embodiment integrates the winding mechanism, the double-sided carbon layer coating mechanism 421, the drying mechanism 422, the first-side coating mechanism 431, the first oven 432, the second-side coating mechanism 441, the second oven 442 and the winding mechanism 45 into a production line, which saves space and reduces the footprint of the equipment; at the same time, through a continuous and efficient production process, it reduces the waste of equipment and human resources and reduces production costs.

[0096] In addition, compared with the related art, the aluminum foil coating process requires two coatings and two windings. In the battery aluminum foil coating device 4 provided in this embodiment, the aluminum foil only needs one unwinding and one winding to achieve double-sided coating of the aluminum foil, which effectively reduces the tediousness of the operation, avoids manual handling of the aluminum foil material, and saves manpower.

[0097] It should be noted that the unwinding mechanism 41, the double-sided carbon layer coating mechanism 421, the drying mechanism 422, the first-side coating mechanism 431, the first oven 432, the second-side coating mechanism 441, the second oven 442 and the winding mechanism 45 can be connected through belt walking, and this embodiment does not impose specific restrictions on the connection method between the above-mentioned mechanisms and / or components.

[0098] See also Figure 3It is a structural schematic diagram of a double-sided coating device for a battery aluminum foil carbon layer in the related art; in the related art, the double-sided coating device 3 includes a unwinding mechanism 31, a first-side coating component 32, a second-side coating component 33 and a winding mechanism 34, wherein the unwinding mechanism 31 is used to unwind the aluminum foil, the first-side coating component 32 is used to sequentially coat the carbon layer slurry and the electrode slurry on the first side of the aluminum foil, and dry the first side of the aluminum foil after coating, the second-side coating component 33 is used to sequentially coat the carbon layer slurry and the electrode slurry on the second side of the aluminum foil, and dry the second side of the aluminum foil after coating, and the winding mechanism 34 is used to wind up the coated aluminum foil; wherein the aluminum foil passes through the unwinding mechanism 31, the first-side coating component 32, the second-side coating component 33 and the winding mechanism 34 in sequence, that is, by combining the aluminum foil carbon layer coating process and the electrode slurry coating process, the production cost is greatly reduced, the production cycle is shortened and the waste of resources is reduced.

[0099] exist Figure 3 In the provided double-sided coating device 3, the carbon coating slurry and the electrode slurry are mixed, and then the carbon coating slurry and the electrode slurry are sequentially coated on the first side of the aluminum foil, and the first side of the aluminum foil after coating is dried, and the carbon coating slurry and the electrode slurry are sequentially coated on the second side of the aluminum foil, and the second side of the aluminum foil after coating is dried, thereby completing the double-sided coating; wherein, in order to achieve the simultaneous drying of the carbon coating slurry and the electrode slurry, the solvent system of the carbon coating slurry and the solvent system of the electrode slurry must be the same, thereby limiting its use conditions.

[0100] It can be understood that the battery aluminum foil coating device 4 in this embodiment includes a double-sided coating component 42, a first-sided coating component 43 and a second-sided coating component 44. The double-sided coating component 42 can be used to coat the carbon coating slurry on both sides of the aluminum foil, and the first and second sides of the coated aluminum foil are dried at the same time, so that the carbon coating layer is formed on the first and second sides of the aluminum foil. Then, the electrode slurry is coated on the carbon coating layer on the first side of the aluminum foil by the first-side coating component 43, and the first side of the coated aluminum foil is dried. The second-side coating component 44 coats the electrode slurry on the carbon coating layer on the second side of the aluminum foil, and bakes the second side of the aluminum foil after coating; wherein, since the present design coats the electrode slurry on the dried carbon coating layer, even if the solvent system of the carbon coating layer slurry is different from the solvent system of the electrode slurry, the two slurries will not be in direct contact, thereby avoiding chemical reactions and incompatibility problems between them; that is, the present embodiment adopts a step-by-step coating technology to allow the use of carbon coating layer slurries and electrode slurries of different systems, thereby reducing the strict requirements for material compatibility.

[0101] It should be noted that, since the electrode slurry is coated on the dried carbon coating layer, the carbon coating layer slurry has no effect on the coating of the electrode slurry. In this embodiment, the solvent system of the carbon coating layer slurry may be different from the solvent system of the electrode slurry, or the solvent system of the carbon coating layer slurry may be the same as the solvent system of the electrode slurry. That is, this embodiment does not impose any specific restrictions on the solvent system of the carbon coating slurry and the solvent system of the electrode slurry.

[0102] Furthermore, in this embodiment, the battery aluminum foil coating device 4 also includes a corona mechanism 46 and a correcting mechanism 47; the corona mechanism 46 is used to remove oil stains on the surface of the aluminum foil before coating; the correcting mechanism 47 is arranged between the drying mechanism 422 and the first-side coating mechanism 431; and / or, the correcting mechanism 47 is arranged between the first oven 432 and the second-side coating mechanism 441; and / or, the correcting mechanism 47 is arranged between the second oven 442 and the winding mechanism 45; the correcting mechanism 47 is used to adjust the aluminum foil tape deviation and coating misalignment.

[0103] Specifically, the deflection correction mechanism 47 includes a first deflection correction structure 471, a second deflection correction structure (not shown in the figure), a third deflection correction structure 473 and a fourth deflection correction structure (not shown in the figure); the first deflection correction structure 471 is located between the corona mechanism 46 and the double-sided coating assembly 42, and the first deflection correction structure 471 is used to detect whether the aluminum foil is misaligned when being conveyed on the belt between the corona mechanism 46 and the double-sided coating assembly 42, and to adjust the foil belt deviation; the second deflection correction structure is located between the drying mechanism 422 and the first-side coating mechanism 431, and the second deflection correction structure is used to detect whether the aluminum foil is misaligned when being conveyed on the belt between the drying mechanism 422 and the first-side coating mechanism 431 1, and adjust the deviation of the aluminum foil tape run; the third correcting structure 473 is located between the first oven 432 and the second-side coating mechanism 441, and the third correcting structure 473 is used to detect whether the aluminum foil is misaligned when it is conveyed on the tape run between the first oven 432 and the second-side coating mechanism 441, and adjust the deviation of the aluminum foil tape run; the fourth correcting structure is located between the second oven 442 and the winding mechanism 45, and the fourth correcting structure is used to detect whether the aluminum foil is misaligned when it is conveyed on the tape run between the second oven 442 and the winding mechanism 45, and adjust the deviation of the aluminum foil tape run.

[0104] It can be understood that this embodiment monitors and adjusts the aluminum foil tape deviation and coating misalignment by setting the first correcting structure 471, the second correcting structure, the third correcting structure 473 and the fourth correcting structure, thereby improving the aluminum foil coating accuracy and stabilizing the aluminum foil travel.

[0105] Please combine Figure 4 and Figure 5 ;in, Figure 5 This is a flow chart of the coating method of battery aluminum foil provided in an embodiment of the present application.

[0106] This embodiment also provides a battery aluminum foil coating method. It should be noted that one embodiment of the battery aluminum foil coating method is to use the above-mentioned battery aluminum foil coating device to coat the aluminum foil, thereby forming a battery electrode to be cut.

[0107] Step S10: After the aluminum foil roll is unrolled by the unwinding mechanism 41 , the aluminum foil is sent to the double-sided coating assembly 42 .

[0108] Specifically, the step S10 includes the following steps:

[0109] Step S11: After the aluminum foil roll is unrolled by the unwinding mechanism 41, the aluminum foil can be sent to the corona mechanism 46 through the guide roller; wherein, the corona mechanism 46 is used to remove oil stains on the surface of the aluminum foil and change the surface energy of the aluminum foil to make it easier to bond with the primer slurry in the subsequent process.

[0110] Step S12: After the aluminum foil roll passes through the corona mechanism 46, the aluminum foil can be sent into the first correcting structure 471 and the double-sided coating component 42 in sequence through the guide roller; wherein the first correcting structure 471 is used to detect whether the aluminum foil is misaligned when being conveyed on the conveyor between the corona mechanism 46 and the double-sided coating component 42, and to adjust the foil conveyor deviation.

[0111] Step S20: the aluminum foil enters the double-sided coating assembly 42, and the double-sided coating assembly 42 is used to first coat the carbon coating slurry on the first side of the aluminum foil, and then coat the carbon coating slurry on the second side of the aluminum foil, and then the first side and the second side of the coated aluminum foil are dried at the same time, and finally the aluminum foil with the carbon coating is sent to the first side coating assembly 43.

[0112] Specifically, in step S20, the following steps are included:

[0113] Step S21 : the aluminum foil enters the first carbon layer coating mechanism 4211 , and the first carbon layer coating mechanism 4211 is used to coat the carbon layer coating slurry on the first surface of the aluminum foil, and then the aluminum foil is sent to the second carbon layer coating mechanism 4212 .

[0114] Specifically, the coating method of the carbon coating slurry includes but is not limited to gravure transfer coating, and the first carbon layer coating mechanism 4211 includes a first gravure coating roller, and the first gravure coating roller drives the aluminum foil to move to coat the first surface of the carbon coating slurry.

[0115] Step S22 : the aluminum foil enters the second carbon layer coating mechanism 4212 , the second carbon layer coating mechanism 4212 is used to coat the carbon layer slurry on the second surface of the aluminum foil, and then the aluminum foil is sent to the drying mechanism 422 .

[0116] Among them, the carbon coating slurry can be an aqueous system, and the carbon coating slurry includes but is not limited to a main powder, a special glue and an organic solvent; wherein, the main powder can be selected from one of carbon black (SP) or graphene (GR), and the special glue can include a polymer binder, such as polyacrylic acid (PAA), polyvinyl alcohol (PVA), polytetrafluoroethylene (PTFE), polyolefins (PP, PE and other copolymers), polyvinylidene fluoride (PVDF), and one of modified SBR rubber, which can form a strong coating after drying, and the organic solvent can be selected from deionized water.

[0117] Specifically, the coating method of the carbon coating slurry includes but is not limited to gravure transfer coating, and the second carbon layer coating mechanism 4212 includes a second gravure coating roller, and the second gravure coating roller drives the aluminum foil to move to coat the second surface with the carbon coating slurry.

[0118] It should be noted that after the carbon coating slurry is coated on the second side of the aluminum foil, the foil detection equipment can be used to complete the carbon coating thickness and defect detection on the first and second sides of the aluminum foil to ensure that the width of the aluminum foil is within the preset specification range and does not exceed the tolerance range. At the same time, any defects on the surface of the aluminum foil are identified, such as bubbles, cracks, uncoated areas, uneven coating, etc.; wherein, after the defects are identified, the defective aluminum foil can be discarded or reworked in the subsequent production process; wherein, this embodiment does not specifically limit the type of foil detection equipment, and this embodiment takes the foil detection equipment as a macro charge coupled device (CCD) camera as an example to illustrate the technical solution of the present application.

[0119] Step S23: the aluminum foil enters the drying mechanism 422 , and the first side and the second side of the coated aluminum foil are dried simultaneously by the drying mechanism 422 , and then the aluminum foil coated with the carbon layer is sent to the first side coating assembly 43 .

[0120] It should be noted that before the aluminum foil enters the drying mechanism 422, since the carbon coating slurry on the first side and the carbon coating slurry on the second side of the aluminum foil are not dried, a smoothing roller can be used to guide the aluminum foil into the drying mechanism 422, so as to control the tension of the aluminum foil during the drying process to ensure that the surface coating of the foil after coating is uniform and free of wrinkles or other defects.

[0121] Specifically, the heat source of the drying mechanism 422 can be at least one of steam, electric heater, infrared, and microwave. The appropriate drying method can be selected according to actual needs to ensure that the coated aluminum foil can be efficiently dried. This embodiment takes the drying mechanism 422 as an infrared oven as an example to illustrate the technical solution of the present application.

[0122] The drying mechanism 422 may include an oven and a plurality of infrared heating elements inside the oven, wherein the plurality of infrared heating elements are respectively installed at the top and the bottom of the oven, and the aluminum foil may be moved inside the oven via a conveyor belt, and the design of the conveyor belt may ensure that the aluminum foil moves smoothly under the infrared heating elements to ensure that both the first side and the second side of the aluminum foil can receive infrared radiation at the same time; at the same time, by adjusting the radiation intensity of the infrared heating elements at the top and the bottom, the uniformity of heating the first side and the second side of the aluminum foil may be controlled.

[0123] The drying temperature range of the drying mechanism 422 is greater than or equal to 70 degrees Celsius and less than or equal to 170 degrees Celsius, and the drying time range of the drying mechanism 422 is greater than or equal to 3 seconds and less than or equal to 9 seconds; wherein, the baking time of the aluminum foil is only related to the speed of the conveyor belt, the faster the speed of the conveyor belt, the shorter the baking time, the speed range of the conveyor belt is greater than or equal to 20 meters / minute and less than or equal to 70 meters / minute, and the length of the drying mechanism is approximately 3 meters.

[0124] Furthermore, after the aluminum foil is dried by the drying mechanism 422, the aluminum foil can be inspected by an area density meter; wherein, the area density meter is an instrument for measuring the quality of the surface coating of a material, and the area density meter can use X-rays (X-ray) or β-rays (β-ray) as a detection means. The area density of the carbon coating layer on the surface of the aluminum foil, that is, the quality of the carbon coating layer per unit area, can be detected by the area density meter, thereby ensuring that the coating is uniform and meets the predetermined specifications and standards.

[0125] It can be understood that in this embodiment, the double-sided coating component 42 can be used to coat the carbon coating slurry on both sides of the aluminum foil respectively, and the first side and the second side of the coated aluminum foil are dried at the same time to evaporate the water or other solvents in the carbon coating slurry, and the carbon coating slurry is dried and adhered to the surface of the aluminum foil, thereby forming a carbon coating layer on both the first side and the second side of the aluminum foil.

[0126] Furthermore, in the step S20, after the aluminum foil is detected by the surface density meter, the aluminum foil can be sent into the second correcting structure and the first-side coating component 43 in sequence by using the conveyor belt; wherein the second correcting structure is used to detect whether the aluminum foil is misaligned when being conveyed on the conveyor belt between the drying mechanism 422 and the first-side coating component 43.

[0127] Step S30: the aluminum foil enters the first-side coating assembly 43, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the first side of the aluminum foil after the carbon coating by the first-side coating assembly 43, and the first side of the aluminum foil after the electrode slurry is coated is dried, and then the aluminum foil is sent to the second-side coating assembly 44.

[0128] Specifically, in step S30, the following steps are included:

[0129] Step S31: the aluminum foil enters the first-side coating mechanism 431 , and the electrode slurry and the ceramic insulating slurry are sequentially coated on the first side of the aluminum foil after the carbon coating by the first-side coating mechanism 431 , and then the aluminum foil is sent to the first oven 432 .

[0130] The electrode slurry can be an oily system, and the electrode slurry includes an active substance, a binder, a dispersant, a conductive agent and an organic solvent, wherein the active substance can be lithium iron phosphate, the binder can be polyvinylidene fluoride, the dispersant can be YTF003, the conductive agent can be carbon nanotubes, and the organic solvent can be N-methylpyrrolidone (NMP); the solvent system of the ceramic insulating slurry is the same as the solvent system of the electrode slurry. Since the two belong to the same system, the ceramic insulating slurry and the electrode slurry can be mutually soluble in each other at their junction, and are convenient for being dried together in the subsequent drying process; it should be noted that this embodiment does not specifically limit the material of the ceramic insulating slurry.

[0131] Furthermore, the viscosity of the electrode slurry is in the range of greater than or equal to 5000 mPa·s and less than or equal to 25000 mPa·s, and the viscosity of the ceramic insulating slurry is in the range of greater than or equal to 1000 mPa·s and less than or equal to 7000 mPa·s; the solid content of the electrode slurry is greater than or equal to 60% and less than or equal to 70%, and the solid content of the ceramic insulating slurry is greater than or equal to 30% and less than or equal to 38%.

[0132] Specifically, the first-surface coating mechanism 431 may include a first die head, which may be divided into two areas, one area for coating the entire surface of the electrode slurry, and the other area for coating the edge of the ceramic insulating slurry; wherein the two areas may be separated by a fluid isolation structure to ensure that the two materials are not mixed in the die head.

[0133] It should be noted that, in the present embodiment, after the electrode slurry and the ceramic insulating slurry are coated on the first side of the aluminum foil by the first side coating mechanism 431, the wet film surface density of the first side of the coated aluminum foil can be detected by using an area density meter, so that problems that may occur in the coating process, such as uneven coating, thickness deviation, etc., can be discovered in time to ensure that each batch of products meets the standards; and, based on the measurement results, the parameters of the coating equipment, such as coating speed, slurry supply, coating pressure, etc., can be adjusted in real time to optimize the coating effect.

[0134] Step S32 : the aluminum foil enters the first oven 432 , the first oven 432 is used to dry the first side of the coated aluminum foil, and then the aluminum foil is sent to the second side coating assembly 44 .

[0135] The drying temperature of the first oven 432 is in the range of greater than or equal to 85 degrees Celsius and less than or equal to 105 degrees Celsius, and the drying time of the aluminum foil in the first oven 432 is in the range of greater than or equal to 2 minutes and less than or equal to 4 minutes.

[0136] Specifically, there is a flowing high-temperature airflow in the first oven 432, and the solvent of the electrode slurry is taken away by the flowing high-temperature airflow, thereby drying the first side of the aluminum foil; it should be noted that the first side of the dried aluminum foil can ensure the stability of the electrode slurry and the ceramic insulating slurry through an airflow cooling system, a tensioning system, a dry film detection system and a correction structure.

[0137] It should be noted that, in the present embodiment, after the aluminum foil is dried by the first oven 432, the surface density of the dry film of the aluminum foil after drying can be detected by using an area density meter, so that problems that may occur in the coating process, such as uneven coating, thickness deviation, etc., can be discovered in time to ensure that each batch of products meets the standards; and, based on the measurement results, the parameters of the coating equipment, such as coating speed, slurry supply, coating pressure, etc., can be adjusted in real time to optimize the coating effect; and, a guide roller or a tension separation roller can be set between the first oven 432 and the second surface coating assembly 44, and the aluminum foil passing through the first oven 432 can be separated from the subsequent process by the guide roller or the tension separation roller, so that the tension at the outlet of the first oven 432 and the subsequent process can be independently controlled to avoid mutual interference.

[0138] It can be understood that combining the electrode slurry coating process of the aluminum foil with the ceramic insulating layer slurry coating process greatly reduces the production cost, shortens the production cycle and reduces resource waste.

[0139] Furthermore, in the step S30, after the aluminum foil is inspected by the surface density meter, the aluminum foil can be sequentially fed into the third correcting structure 473 and the second electrode slurry coating machine by means of the belt conveyor, wherein the third correcting structure 473 is used to detect whether the aluminum foil is misaligned when being transported on the belt conveyor between the first oven 432 and the second surface coating mechanism 441, and to adjust the belt conveyor offset of the aluminum foil.

[0140] Step S40: the aluminum foil enters the second-side coating assembly 44, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the second side of the aluminum foil after the carbon coating by the second-side coating assembly 44, and the second side of the aluminum foil after the electrode slurry is coated is dried, and then the aluminum foil is sent to the winding mechanism 45.

[0141] Specifically, in step S40, the following steps are included:

[0142] Step S41: the aluminum foil enters the second-side coating mechanism 441 , and the electrode slurry and the ceramic insulating slurry are sequentially coated on the second side of the aluminum foil after the carbon coating is completed by the second-side coating mechanism 441 , and then the aluminum foil is sent to the second oven 442 .

[0143] Specifically, the coating method of the electrode slurry includes but is not limited to one of transfer coating, extrusion coating or wet coating; the second surface coating mechanism 441 may include a second die head, and the second die head may be divided into two areas, one area is used for the entire surface coating of the electrode slurry, and the other area is used for the edge coating of the ceramic insulating slurry; wherein the two areas can be separated by a fluid isolation structure to ensure that the two materials are not mixed in the die head.

[0144] It should be noted that, in the present embodiment, after the electrode slurry and the ceramic insulating slurry are coated on the second side of the aluminum foil by the second side coating mechanism 441, the wet film surface density of the second side of the aluminum foil coated with the electrode slurry can be detected by using a surface density meter, so that problems that may occur in the coating process, such as uneven coating, thickness deviation, etc., can be discovered in time to ensure that each batch of products meets the standards; and, based on the measurement results, the parameters of the coating equipment, such as coating speed, slurry supply, coating pressure, etc., can be adjusted in real time to optimize the coating effect.

[0145] Step S42: the aluminum foil enters the second oven 442, the second oven 442 is used to dry the second surface of the coated aluminum foil, and then the coated aluminum foil is introduced into the winding mechanism 45 through the guide roller.

[0146] The drying temperature of the second oven 442 is in the range of greater than or equal to 90 degrees Celsius and less than or equal to 115 degrees Celsius, and the drying time of the aluminum foil in the second oven 442 is in the range of greater than or equal to 2 minutes and less than or equal to 4 minutes.

[0147] Specifically, the second oven 442 has a flowing high-temperature airflow, and the solvent of the electrode slurry is taken away by the flowing high-temperature airflow, thereby drying the second side of the aluminum foil; it should be noted that the second side of the dried aluminum foil can ensure the stability of the electrode slurry and the ceramic insulating slurry through an airflow cooling system, a tensioning system, a dry film detection system and a correction structure.

[0148] It can be understood that in this embodiment, the electrode slurry is coated on the carbon coating layer on the first side of the aluminum foil through the first-side coating component 43, and the first side of the aluminum foil after coating is baked, and the electrode slurry is coated on the carbon coating layer on the second side of the aluminum foil through the second-side coating component 44, and the second side of the aluminum foil after coating is baked; wherein, since the present design is to coat the electrode slurry on the dried carbon coating layer, even if the solvent system of the carbon coating layer slurry is different from the solvent system of the electrode slurry, the two slurries will not directly contact each other, thereby avoiding chemical reactions and incompatibility problems between them; that is, the present embodiment adopts a step-by-step coating technology to allow the use of carbon coating layer slurries and electrode slurries of different systems, thereby reducing the strict requirements for material compatibility.

[0149] It should be noted that the carbon coating slurry is an aqueous system, and the electrode slurry is an oily system. The solvent system of the carbon coating layer slurry is different from the solvent system of the electrode slurry and is only used for illustration. In the present embodiment, since the electrode slurry is coated on the dried carbon coating layer, the carbon coating layer slurry has no effect on the coating of the electrode slurry. Therefore, the solvent system of the carbon coating layer slurry may be the same as the solvent system of the electrode slurry. For example, the solvent of the carbon coating layer slurry and the electrode slurry may both be oily systems. That is, the present embodiment does not impose any specific restrictions on the solvent system of the carbon coating slurry and the solvent system of the electrode slurry.

[0150] Please combine Figure 6 and Figure 7 ;in, Figure 6 A top view of the battery aluminum foil provided in the embodiment of the present application after the double-sided coating process is completed; Figure 7 This is a schematic diagram of the structure of the coating main layer provided in an embodiment of the present application.

[0151] It should be noted that Figure 6 It may be a top view of the first surface of the aluminum foil or a top view of the second surface of the aluminum foil, and this embodiment does not impose any specific limitation on this.

[0152] The aluminum foil includes a coating layer 51 and a foil portion 52 . The coating layer 51 includes a coating main layer 511 and a ceramic insulating layer 512 . The coating main layer 511 includes a stacked carbon coating layer 5111 and an electrode layer 5112 . The ceramic insulating layer 512 is located between the coating main layer 511 and the foil portion 52 .

[0153] Among them, since the present embodiment combines the electrode slurry coating process and the ceramic insulating layer slurry coating process of the aluminum foil, the solvent system of the ceramic insulating layer slurry is the same as the solvent system of the electrode slurry. Therefore, when the electrode slurry and the ceramic insulating layer slurry are sequentially coated on the first side of the aluminum foil, a contact fusion layer exists between the electrode slurry and the ceramic insulating layer slurry. Since the carbon layer coating process and the electrode slurry coating process are completed separately, when the electrode slurry is coated on the first side of the aluminum foil, the carbon layer slurry has been dried. Therefore, on the first side of the aluminum foil, there is no contact fusion layer between the electrode slurry and the carbon layer slurry.

[0154] There is an overlapping portion P between the ceramic insulating layer 512 and the coating layer 51, and the overlapping portion P is a contact fusion layer between the electrode slurry and the ceramic insulating layer slurry. The overlapping portion P points in the direction of the coating layer 51, and the width range of the overlapping portion P is greater than 0 and less than or equal to 0.5 mm; the width range of the ceramic insulating layer 512 is greater than or equal to 2.6 mm and less than or equal to 3.2 mm.

[0155] Furthermore, in the step S40, after the aluminum foil is dried by the second oven 442, the aluminum foil can be sequentially fed into the fourth deflection correction structure and the winding mechanism 45 using the belt conveyor, wherein the fourth deflection correction structure is used to detect whether the aluminum foil is deflected when being transported on the belt conveyor between the second oven 442 and the winding mechanism 45, and to adjust the deflection of the aluminum foil belt conveyor.

[0156] Step S50: The aluminum foil is rolled up by the rolling mechanism 45 to complete the coating of the aluminum foil.

[0157] It can be understood that this embodiment saves space and reduces the footprint of equipment by integrating the rolling mechanism, the double-sided carbon layer coating mechanism 421, the drying mechanism 422, the first-side coating mechanism 431, the first oven 432, the second-side coating mechanism 441, the second oven 442 and the winding mechanism 45 into a production line; at the same time, through a continuous and efficient production process, the production cost is greatly reduced, the production cycle is shortened, the waste of resources is reduced, the waste of equipment and human resources is reduced, and the production cost is reduced.

[0158] Further, please refer to the following comparative example 1, which is a coating method of battery aluminum foil in the related art.

[0159] Comparative Example 1:

[0160] The coating method of the battery aluminum foil of this comparative example 1 comprises the following steps:

[0161] D10: The aluminum foil is sequentially fed into the aluminum foil unwinding mechanism 41, the aluminum foil corona mechanism 46, the aluminum foil first side carbon layer coating mechanism, the first aluminum foil oven, the aluminum foil second side carbon layer coating mechanism, the second aluminum foil oven and the first aluminum foil winding mechanism 45, thereby completing the double-sided carbon layer coating process of the aluminum foil.

[0162] Specifically, in the related art, the carbon layer coating speed ranges from 180 m / min to 200 m / min, the temperature range of the first aluminum foil oven is 85 degrees Celsius to 105 degrees Celsius, and the drying time of the first side of the aluminum foil in the first aluminum foil oven is 0.1 minute; the coating speed of the second side of the aluminum foil is consistent with the coating speed of the second side of the aluminum foil. When the carbon layer is coated on 10,000 meters of aluminum foil, it takes at least 50 minutes; among them, the winding and transportation time is time-consuming, and many factories need to separate the factory that completes the carbon layer coating from the factory that completes the electrode slurry coating. The time consumed by the aluminum foil during transportation takes at least 30 minutes.

[0163] D20: The aluminum foil that has completed the double-sided carbon layer coating process is sequentially sent to the second aluminum foil unwinding mechanism 41, the aluminum foil first side electrode slurry coating mechanism, the third aluminum foil oven, the aluminum foil second side electrode slurry coating mechanism, the fourth aluminum foil oven and the second aluminum foil winding mechanism 45, thereby completing the double-sided electrode slurry coating process of the aluminum foil.

[0164] Specifically, in the related art, the electrode slurry coating speed is 40 m / min, the drying time of the first side of the aluminum foil in the first aluminum foil oven is in the range of 2 minutes to 4 minutes, and the drying time of the second side of the aluminum foil in the second aluminum foil oven is in the range of 2 minutes to 4 minutes.

[0165] From the above content, it can be seen that in Comparative Example 1, the carbon layer coating process and the electrode slurry coating process are completed separately; wherein, the time for completing the carbon layer coating process on both sides of the aluminum foil includes:

[0166] The time for carbon coating on the first side of the aluminum foil, the time for drying the slurry of the carbon layer coated on the first side of the aluminum foil, the time for carbon coating on the second side of the aluminum foil, the time for drying the slurry of the carbon layer coated on the second side of the aluminum foil, the time for transporting the aluminum foil with double-sided carbon coating from the carbon layer coating factory to the electrode slurry coating factory, the time for coating the first side of the aluminum foil with electrode slurry, the time for drying the electrode slurry on the first side of the aluminum foil, the time for coating the second side of the aluminum foil with electrode slurry, and the time for drying the slurry of the electrode slurry layer on the second side of the aluminum foil; specifically, in the related art, it takes at least 330 minutes for the aluminum foil to complete the double-sided carbon layer coating process and the double-sided electrode slurry coating process.

[0167] By comparison, it can be seen that in the coating method of battery aluminum foil provided in the embodiment, the aluminum foil passes through the unwinding mechanism, the double-sided carbon layer coating mechanism 421, the drying mechanism, the first-side coating mechanism 431, the first oven 432, the second-side coating mechanism 441, the second oven 442 and the winding mechanism 45 in sequence, so that the aluminum foil can be double-sided coated with only one unwinding and one winding, which effectively reduces the cumbersomeness of the operation, avoids manual handling of the aluminum foil material, and saves manpower; and, by integrating the process of coating the carbon layer slurry and the process of coating the motor slurry on one production line, while saving the time of transporting the double-sided carbon layer coated aluminum foil from the carbon layer coating factory to the electrode slurry coating factory, the production cost is greatly reduced, the production cycle is shortened, the waste of resources is reduced, and the land space is saved.

[0168] See also Figure 8 , which is a schematic diagram of the structure of the current collector provided in an embodiment of the present application.

[0169] The embodiment of the present application further provides a current collector 5, wherein the current collector 5 comprises an aluminum foil, and the aluminum foil can be manufactured by using the above-mentioned coating method of the battery aluminum foil.

[0170] Specifically, the current collector 5 includes a metal layer 53 and a coating layer 51 provided on both sides of the metal layer 53; wherein the metal layer 53 may be an aluminum foil, the coating layer 51 includes a stacked carbon coating layer 5111 and an electrode layer 5112, and the coating layer 51 may be coated on the aluminum foil using the above-mentioned coating method for the battery aluminum foil; it should be noted that the coating method for the battery aluminum foil has been described in detail in the above-mentioned embodiment and will not be repeated here.

[0171] It can be understood that the current collector 5 adopts a double-sided coating process of carbon coating slurry and electrode slurry, which can significantly improve the conductivity of the aluminum foil surface. Among them, the addition of the carbon coating layer 5111 provides the current collector with excellent static conductivity, which can more effectively collect the microcurrent generated in the electrode material and improve the conductivity of the battery, which has a positive effect on the battery's charging and discharging efficiency, cycle life and overall battery performance. In addition, the solvent system of the carbon coating slurry is different from the solvent system of the electrode slurry, which improves the flexibility of material selection and makes the process no longer limited to the use of materials of the same system, which helps to develop battery structures that are more suitable for a variety of application scenarios and expands the application scope of the technology.

[0172] Please combine Figure 8 and Fig. 9 ;in, Fig. 9 A schematic diagram of the structure of a battery provided in an embodiment of the present application.

[0173] This embodiment further provides a battery 6, which includes a positive electrode sheet 61 and a negative electrode sheet 62, wherein the positive electrode sheet 61 includes a positive electrode current collector and a positive electrode active material, and the negative electrode sheet 6 includes a negative electrode current collector; wherein at least one of the positive electrode current collector and the negative electrode current collector can be the current collector described in any of the above embodiments.

[0174] Specifically, the battery 6 includes a positive electrode sheet 61, a negative electrode sheet 62, and a separator 63 arranged between the positive electrode sheet 61 and the negative electrode sheet 62; wherein the positive electrode sheet, the negative electrode sheet 62, and the separator 63 can be a laminated battery cell or a wound battery cell, and the battery 6 includes but is not limited to one of a soft-pack battery, a square battery, or a cylindrical battery.

[0175] It should be noted that, in this embodiment, the electrode slurry is taken as an example to illustrate the technical solution of the present application, that is, in this embodiment, the positive electrode current collector is the current collector described in any of the above embodiments.

[0176] It can be understood that the current collector can be used as a core component of the positive and negative electrodes in the battery, directly affecting the charge and discharge performance, energy density and cycle life of the battery. This embodiment can greatly improve the conductivity and mechanical properties of the current collector by double-sided coating of the carbon layer slurry and the electrode slurry, thereby providing more stable and efficient support for the battery, thereby improving the overall performance of the battery.

[0177] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0178] The above is a detailed introduction to a battery aluminum foil coating device and coating method, a current collector and a battery provided in this embodiment. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A battery aluminum foil coating device, characterized in that: include: Unwinding mechanism, used for unwinding aluminum foil; A double-sided coating assembly is used to first coat the carbon coating slurry on the first side of the aluminum foil, then coat the carbon coating slurry on the second side of the aluminum foil, and finally dry the coated first side and second side of the aluminum foil simultaneously; A first-side coating assembly is used to sequentially coat the electrode slurry and the ceramic insulating slurry on the first side of the aluminum foil, and dry the coated first side of the aluminum foil; A second side coating assembly is used to sequentially coat the electrode slurry and the ceramic insulating slurry on the second side of the aluminum foil, and dry the coated second side of the aluminum foil; The winding mechanism is used to wind up the coated aluminum foil; The aluminum foil passes through the unwinding mechanism, the double-sided coating assembly, the first-sided coating assembly, the second-sided coating assembly and the winding mechanism in sequence to complete double-sided coating.

2. The battery aluminum foil coating device according to claim 1, characterized in that: The double-sided coating assembly is located between the unwinding mechanism and the first-sided coating assembly, and the double-sided coating assembly includes a double-sided carbon layer coating mechanism and a drying mechanism connected in sequence; The first-side coating assembly is located between the double-side coating assembly and the second-side coating assembly, the first-side coating assembly includes a first-side coating mechanism and a first oven connected in sequence, and the second-side coating assembly includes a second-side coating mechanism and a second oven connected in sequence.

3. The battery aluminum foil coating device according to claim 2, characterized in that: The double-sided carbon layer coating mechanism comprises: Frame; A first carbon layer coating mechanism, used for coating a carbon layer coating slurry on a first surface of the aluminum foil; A second carbon layer coating mechanism, used for coating a carbon layer slurry on the second surface of the aluminum foil; Wherein, the first carbon layer coating mechanism and the second carbon layer coating mechanism are both located in the frame, and the aluminum foil passes through the first carbon layer coating mechanism and the second carbon layer coating mechanism in sequence.

4. The battery aluminum foil coating device according to claim 2, characterized in that: The battery aluminum foil coating device further includes a deviation correction mechanism, which is arranged between the unwinding mechanism and the double-sided coating assembly; And / or, the deviation correcting mechanism is arranged between the drying mechanism and the first-side coating mechanism; And / or, the deviation correction mechanism is arranged between the first oven and the second surface coating mechanism; And / or, the deviation correcting mechanism is arranged between the second oven and the winding mechanism.

5. A coating method for battery aluminum foil, characterized in that: The coating method of the battery aluminum foil comprises at least the following steps: After the aluminum foil roll is unrolled by the unwinding mechanism, the aluminum foil is fed into the double-sided coating assembly; The aluminum foil enters the double-sided coating assembly, and the double-sided coating assembly first coats the carbon coating slurry on the first side of the aluminum foil, and then coats the carbon coating slurry on the second side of the aluminum foil, and then dries the first side and the second side of the coated aluminum foil at the same time, and finally sends the aluminum foil with the carbon coating to the first side coating assembly; The aluminum foil enters the first-side coating assembly, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the first side of the aluminum foil after the carbon coating is completed by the first-side coating assembly, and the first side of the aluminum foil coated with the electrode slurry is dried, and then the aluminum foil is sent to the second-side coating assembly; The aluminum foil enters the second side coating assembly, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the second side of the aluminum foil after the carbon coating is completed by the second side coating assembly, and the second side of the aluminum foil coated with the electrode slurry is dried, and then the aluminum foil is sent to the winding mechanism; The aluminum foil is rolled up by a rolling mechanism to complete the coating of the aluminum foil.

6. The coating method according to claim 5, characterized in that: The aluminum foil enters the double-sided coating assembly, the double-sided coating assembly is used to first coat the carbon coating slurry on the first side of the aluminum foil, then coats the carbon coating slurry on the second side of the aluminum foil, then simultaneously dries the coated first side and second side of the aluminum foil, and finally guides the aluminum foil into the first side coating assembly through a guide roller, the steps comprising: The aluminum foil enters the first carbon layer coating mechanism, the first carbon layer coating mechanism is used to coat the carbon layer coating slurry on the first surface of the aluminum foil, and then the aluminum foil is sent to the second carbon layer coating mechanism; The aluminum foil enters the second carbon layer coating mechanism, the second carbon layer coating mechanism is used to coat the carbon layer slurry on the second surface of the aluminum foil, and then the aluminum foil is sent to the drying mechanism; The aluminum foil enters the drying mechanism, and the first side and the second side of the coated aluminum foil are dried simultaneously by the drying mechanism, and then the aluminum foil coated with the carbon layer is sent to the first side coating assembly.

7. The coating method according to claim 6, characterized in that: The aluminum foil enters the first-side coating assembly, and the first-side coating assembly is used to sequentially coat the first side of the aluminum foil after the carbon coating with the electrode slurry and the ceramic insulation slurry, and the first side of the aluminum foil after the electrode slurry is coated is dried, and then the aluminum foil is fed into the second-side coating assembly. The steps include: The aluminum foil enters the first side coating mechanism, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the first side of the aluminum foil after the carbon coating is completed by the first side coating mechanism, and then the aluminum foil is sent to the first oven; The aluminum foil enters the first oven, the first oven is used to dry the first side of the coated aluminum foil, and then the aluminum foil is sent to the second side coating assembly.

8. The coating method according to claim 7, characterized in that: The aluminum foil enters the second-side coating assembly, and the second-side coating assembly is used to sequentially coat the electrode slurry and the ceramic insulating slurry on the second side of the aluminum foil after the carbon coating is completed, and the second side of the aluminum foil coated with the electrode slurry is dried, and then the aluminum foil is sent to the winding mechanism. The steps include: The aluminum foil enters the second side coating mechanism, and the electrode slurry and the ceramic insulating slurry are sequentially coated on the second side of the aluminum foil after the carbon coating is completed by the second side coating mechanism, and then the aluminum foil is sent to the second oven; The aluminum foil enters the second oven, the second side of the coated aluminum foil is dried by the second oven, and then the aluminum foil is sent to the winding mechanism.

9. The coating method according to claim 8, characterized in that: The drying temperature of the drying mechanism is in the range of greater than or equal to 70 degrees Celsius and less than or equal to 170 degrees Celsius, and the drying time of the drying mechanism is in the range of greater than or equal to 3 seconds and less than or equal to 9 seconds; The drying temperature of the first oven is in the range of greater than or equal to 85 degrees Celsius and less than or equal to 105 degrees Celsius, and the drying time of the aluminum foil in the first oven is in the range of greater than or equal to 2 minutes and less than or equal to 4 minutes; The drying temperature of the second oven is in the range of greater than or equal to 90 degrees Celsius and less than or equal to 115 degrees Celsius, and the drying time of the aluminum foil in the second oven is in the range of greater than or equal to 2 minutes and less than or equal to 4 minutes.

10. The coating method according to claim 5, characterized in that: The solvent system of the carbon coating slurry is different from the solvent system of the electrode slurry.

11. A current collector, characterized in that: It comprises an aluminum foil, and the aluminum foil is made by the coating method of battery aluminum foil according to any one of claims 5 to 10.

12. A battery, characterized in that: It includes a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet includes a positive electrode current collector and a positive electrode active material, and the negative electrode sheet includes a negative electrode current collector; Wherein, at least one of the positive electrode current collector and the negative electrode current collector is the current collector as claimed in claim 11.

Citation Information

Patent Citations

  • Positive plate and preparation method and application thereof

    CN112701249A

  • Power lithium cell all -in -one

    CN207909997U

  • Micro-gravure coating mechanism capable of coating two surfaces at one time

    CN217528025U

Cited By

  • Precise coating forming method for lithium ion battery pole piece

    CN120895601A

  • Lithium ion battery positive pole piece and preparation method thereof

    CN122659048A

  • A lithium ion battery positive electrode sheet and a preparation method thereof

    CN122659048B