Dual-scale super-hydrophobic coating and preparation method thereof
By spraying PFA powder on the substrate surface to form a micro and nano double-scale structure, the problem that superhydrophobic coatings in the prior art is difficult to achieve high durability and superhydrophobicity on a large area, and high efficiency and low cost double-scale super-scale Hydrophobic coating is prepared, with excellent mechanical stability and superhydrophobic properties.
Patent Information
- Application Number
- CN202411335321.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
The existing superhydrophobic coating technology is difficult to achieve high durability and superhydrophobicity on a large area at the same time, and the preparation process is complex and cannot adapt to large-scale production.
PFA powder is used as filler and binder, and micro and nano-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-bino-b
It realizes a coating with high durability and superhydrophobicity on a large area. It has simple process and low cost. It has self-cleaning, anti-aging and low friction characteristics, which enhances the mechanical stability and superhydrophobicity of the coating.
Smart Images

Figure CN119056727A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of self-cleaning coatings, and in particular to a dual-scale super-hydrophobic coating and a preparation method thereof. Background Art
[0002] Research on the surface structure of hydrophobic materials in nature, such as lotus leaves and feathers, shows that super-hydrophobic coatings are composed of rough structures and low surface energy chemicals provided by the surface microstructure. At present, researchers have conducted a lot of research on the preparation methods and applications of super-hydrophobic coatings. The preparation methods of super-hydrophobic surfaces mainly include vapor deposition, photolithography, template method, etc. However, there are still many shortcomings in the current methods. For example, the coating prepared by the template method only has the characteristics of a single scale, and it is impossible to simultaneously ensure the high durability and super-hydrophobicity of the coating. Moreover, this method can only prepare small-area samples, and cannot be used for large-area preparation.
[0003] The dual-scale superhydrophobic coating can rely on its micron-scale structure to improve the overall high durability of the coating; it can rely on its nanoscale structure to lock in more air, making the contact area between the coating surface and water smaller, thereby improving the superhydrophobicity of the coating surface.
[0004] In summary, the development of a superhydrophobic coating that has both high durability and superhydrophobicity, a simple preparation process, and is suitable for large-area preparation has great application potential. Summary of the invention
[0005] In order to overcome the above technical problems, the object of the present invention is to provide a dual-scale super-hydrophobic coating and a preparation method thereof, wherein the method uses molten PFA as a binder and unmelted PFA powder as a filler to solidify on the substrate surface, and establishes a surface dual-scale microstructure through the unmelted PFA powder; and has the characteristics of high durability and super-hydrophobicity. In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0006] A method for preparing a dual-scale super-hydrophobic drag-reducing coating comprises the following steps:
[0007] S1, sending the substrate into a box-type furnace for heating;
[0008] S2, taking out the substrate after step S1, and immediately spraying PFA powder on the substrate;
[0009] S3. After natural cooling, the excess powder on the surface is blown away with a dust removal gun to obtain a dual-scale semi-molten coating, i.e., a dual-scale super-hydrophobic drag-reducing coating.
[0010] The substrate in S1 is stainless steel (Cr22NiMo3N).
[0011] In the step S1, the substrate is heated to 350-440° C. in a box furnace. The function and purpose of this step is to melt and solidify the PFA powder sprayed on the surface of the substrate.
[0012] In the step S2, the PFA powder contains microstructures of micro and nano scales, with average particle sizes of 30-80 μm and 50-200 nm, respectively, and is sprayed until there is unmelted powder on the surface.
[0013] In the step S2, the spraying equipment used is an electrostatic powder spraying equipment.
[0014] The stainless steel is cleaned and dried before spraying.
[0015] The spraying voltage is 60-90kV, because too high a voltage can easily cause powder rebound and edge pitting, and too low a voltage can result in a low powder coating rate; the current is 10-20μA, because too high a current can easily cause discharge to break through the powder coating, and too low a current can result in a low powder coating rate; the spraying distance is 15-30cm, because too close a distance from the spray gun nozzle to the workpiece can easily cause discharge to break through the powder coating, and too far a distance can increase the powder usage and reduce production efficiency.
[0016] The dual-scale super-hydrophobic drag-reducing coating has microstructures of both micro and nano scales. Specifically, nano particles are wrapped on the surface of micro particles, and micro particles are combined in the molten layer.
[0017] When the coating is subjected to external friction, since the diameter of micron particles is larger than that of nanoparticles, the bonding area between micron particles and the molten layer is larger, so the overall bonding force of the coating can be improved, which is beneficial to improving the durability of the coating. The gaps between nanoparticles form air cavities, which have irregular shapes and are randomly distributed on the coating surface to further increase the surface roughness, thereby reducing the solid-liquid contact area and increasing the gas-liquid contact area, thereby improving the overall superhydrophobicity of the coating.
[0018] Beneficial effects of the present invention:
[0019] Micro- and nanostructures can reduce the contact area between droplets and the coating surface. The surface of the coating of the present invention presents a dual-scale microstructure. The nanoscale microstructure enables the surface to have a larger contact angle and a smaller contact hysteresis, and the micrometer-scale microstructure can better adhere to the surface and has better wear resistance. Therefore, the present invention has better wear resistance while ensuring its super-hydrophobicity.
[0020] The present invention uses a one-step spraying method, has simple process, low cost and can be prepared on a large scale.
[0021] Thanks to the corrosion resistance and low surface energy of PFA materials, the coating of the present invention is not only self-cleaning, but also has the advantages of corrosion resistance, aging resistance, low friction coefficient, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a microscopic morphology of the cross section of the coating prepared in the present invention.
[0023] Figure 2 This is a microscopic morphology diagram of the dual-scale structure of the present invention.
[0024] Figure 3 is the contact angle of the surface of Example 1, Example 2 and Example 3 in the present invention.
[0025] Figure 4 Schematic diagram of sandpaper polishing of the test sample in the present invention.
[0026] Figure 5 This is a distance-contact angle diagram of Example 3 of the present invention after sandpaper polishing.
[0027] Figure 6 This is a test diagram of the cross-cut method in Example 3 of the present invention. DETAILED DESCRIPTION
[0028] The present invention will be further described in detail below in conjunction with the accompanying drawings.
[0029] Example 1
[0030] The preparation method of the super hydrophobic drag reducing coating comprises the following steps:
[0031] (1) Substrate pretreatment: The stainless steel was polished with coarse sandpaper, then ultrasonically cleaned with ethanol, rinsed with deionized water, and dried;
[0032] (2) The pretreated stainless steel is placed in a box furnace and heated to 380°C before being taken out;
[0033] (3) using an electrostatic spraying device to spray PFA powder having a particle size of about 60 μm onto the substrate just taken out in step (2) until there is unmelted PFA powder on the surface;
[0034] (4) After the sample has cooled, use a dust removal gun to blow away excess powder on the surface to obtain a semi-molten coating.
[0035] Example 2
[0036] The preparation method of the super hydrophobic drag reducing coating comprises the following steps:
[0037] (1) Substrate pretreatment: The stainless steel was polished with coarse sandpaper, then ultrasonically cleaned with ethanol, rinsed with deionized water, and dried;
[0038] (2) The pretreated stainless steel is placed in a box furnace and heated to 380°C before being taken out;
[0039] (3) using an electrostatic spraying device to spray the mixed PFA powder (60 μm: 100 nm = 1:1) onto the substrate just taken out in step (2) until there is unmelted PFA powder on the surface;
[0040] (4) After the sample has cooled, use a dust removal gun to blow away excess powder on the surface to obtain a semi-molten coating.
[0041] Example 3
[0042] The preparation method of the super hydrophobic drag reducing coating comprises the following steps:
[0043] (1) Substrate pretreatment: The stainless steel was polished with coarse sandpaper, then ultrasonically cleaned with ethanol, rinsed with deionized water, and dried;
[0044] (2) The pretreated stainless steel is placed in a box furnace and heated to 380°C before being taken out;
[0045] (3) using an electrostatic spraying device to spray PFA powder having a particle size of about 100 nm onto the substrate just taken out in step (2) until there is unmelted PFA powder on the surface;
[0046] (4) After the sample has cooled, use a dust removal gun to blow away excess powder on the surface to obtain a fully molten coating.
[0047] Performance Testing:
[0048] Microscopic morphology: Figure 1 It can be seen that the coating is in a semi-molten state. During the coating preparation process, the substrate is first placed in a furnace for heating. Since the spray powder is not pre-heated during the spraying process, there will be heat loss from the substrate to the coating surface during the heat conduction process. This heat loss causes a temperature gradient to form between the substrate surface and the coating surface. In other words, the temperature of the substrate is higher, and the temperature of the substrate surface is greater than the melting point of PFA, so the PFA powder will melt and solidify on the substrate surface, while the temperature of the coating surface is lower, and the temperature of the coating surface is lower than the melting point of PFA, so there will be a layer of unmelted powder. The melted layer will bond the unmelted powder particles to the coating surface. At this time, the molten PFA is equivalent to a binder, which bonds the unmelted powder to the surface, and uses unmelted powder particles to establish a super-hydrophobic surface microstructure. According to the super-hydrophobic Cassie theoretical model:
[0049] cosθ * =f s (cosθ γ +1)-1
[0050] Where: θ * is the apparent contact angle, θ γ is the intrinsic contact angle, f s is the contact area between the solid and liquid on the surface. Assuming that the papilla radius of the superhydrophobic rough structure is r, the relationship between the microstructure and the contact angle is cosθ * ~r 2 (cosθ γ +1)-1, if the coating surface is subjected to shear force F, the relationship between microstructure and stress is From the theory, it can be seen that the contact angle is inversely proportional to the radius r of the papilla, and the mechanical stability of the coating is proportional to the radius, so the superhydrophobicity and mechanical stability of the superhydrophobic surface are trade-offs. Therefore, the preparation of micro- and nano-scale superhydrophobic coatings can make the superhydrophobic coating have both superhydrophobicity and mechanical stability.
[0051] Figure 2 It can be seen that the prepared coating microstructure is an ideal micro-nano dual-scale papillary structure. Specifically, nano-scale particles are evenly dispersed and tightly wrapped on the surface of micron-scale particles, forming a unique micro-nano composite structure. When the coating is subjected to external friction, the micron-scale particles are tightly combined in the molten layer, which can improve the overall binding force of the coating and help improve the mechanical stability of the coating. Since the droplets are in direct contact with the nanoparticle-level particles, the papillary radius of the solid-liquid contact is much smaller than that of the micron-scale particles. According to the above theory, the introduction of nano-scale particles can increase the contact angle of the coating and improve the overall superhydrophobicity of the coating.
[0052] In summary, the micro- and nano-scale dual-scale structure can simultaneously give the superhydrophobic surface excellent mechanical stability and superhydrophobicity.
[0053] Contact angle: Figure 3 It can be seen that the contact angles of Example 1, Example 2 and Example 3 are 135.9°, 148.6° and 155.3°, respectively. Example 1 is a PFA powder spray with an average particle size of 50 μm, and the surface presents a micron-scale structure, so the contact angle is relatively low. Example 2 is a PFA powder spray with an average particle size of 100 nm, and the surface presents a nanoparticle structure. Example 3 is a 50 μm: 100 nm = 1:1 mixed PFA powder spray, and the surface has a dual-scale super-hydrophobic structure, which has the highest contact angle and the best durability.
[0054] Abrasion resistance, adhesion: Place a sample with a diameter of 25 mm and a height of 8 mm on 400-grit sandpaper and place a 200-g weight on it to apply pressure (such as Figure 4 ), and then test the effect of the distance of wear on the sandpaper on the contact angle. Figure 5It can be seen that after being worn by sandpaper, the coating still has a high contact angle and has good wear resistance. The adhesion of the coating was tested by the cross-hatch method. Figure 6 It can be seen that the adhesion of the coating is level 0, which has excellent adhesion.
[0055] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a dual-scale super-hydrophobic drag-reducing coating, characterized in that: The following steps are involved: S1, sending the substrate into a box-type furnace for heating; S2, taking out the substrate after step S1, and immediately spraying PFA powder on the substrate; S3. After natural cooling, the excess powder on the surface is blown away with a dust removal gun to obtain a dual-scale semi-molten coating, i.e., a dual-scale super-hydrophobic drag-reducing coating.
2. The method for preparing a dual-scale super-hydrophobic drag-reducing coating according to claim 1, characterized in that: The substrate in S1 is stainless steel (Cr22NiMo3N).
3. The method for preparing a dual-scale super-hydrophobic drag-reducing coating according to claim 1, characterized in that: In the step S1, the substrate is heated to 350-440° C. in a box furnace.
4. The method for preparing a dual-scale super-hydrophobic drag-reducing coating according to claim 1, characterized in that: In the step S2, the PFA powder contains microstructures of micro and nano scales, with average particle sizes of 30-80 μm and 50-200 nm, respectively, and is sprayed until there is unmelted powder on the surface.
5. The method for preparing a dual-scale super-hydrophobic drag-reducing coating according to claim 1, characterized in that: In the step S2, the spraying equipment used is an electrostatic powder spraying equipment.
6. The method for preparing a dual-scale super-hydrophobic drag-reducing coating according to claim 1, characterized in that: The spraying voltage is 60-90 kV, the current is 10-20 μA, and the spraying distance is 15-30 cm.
7. A dual-scale super hydrophobic drag reduction coating prepared by the method according to any one of claims 1 to 6, characterized in that: It has microstructures of both micro and nano scales, with nano particles wrapped on the surface of micro particles, and micro particles combined in the molten layer; When the coating is subjected to external friction, since the diameter of micron particles is larger than that of nanoparticles, the bonding area between micron particles and the molten layer is larger, which can improve the overall bonding force of the coating and help improve the durability of the coating. The gaps between nanoparticles form air cavities, which have irregular shapes and are randomly distributed on the coating surface to further increase the surface roughness, thereby reducing the solid-liquid contact area and increasing the gas-liquid contact area, thereby improving the overall superhydrophobicity of the coating.