Straightening method of thin 50 steel and application of straightening method

The straightening method for thin-gauge 50 steel addresses bending issues by optimizing temperature and reduction parameters, enhancing production efficiency and reducing post-processing needs.

CN119056909APending Publication Date: 2024-12-03SGIS SONGSHAN CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411386408.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Thin-gauge 50 steel plates experience bending issues during production due to inconsistent temperature and cooling rates, leading to increased post-processing costs and reduced efficiency.

Method used

A straightening method for thin-gauge 50 steel plates involving specific temperature and reduction parameters, including starting straightening temperatures between 820-890°C, total straightening reductions of 0.8-1.2mm, upper cooling bed temperatures ≤670°C, and controlled roller speeds and pressures, with tailored passes and no cooling water application.

Benefits of technology

Effectively prevents bending of 50 steel plates, reducing the need for reworking and improving production efficiency by controlling deformation stress and minimizing cooling bed wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056909A_ABST
    Figure CN119056909A_ABST
Patent Text Reader

Abstract

The invention discloses a straightening method for thin 50 steel and application of the straightening method, and relates to the technical field of steel production. Comprising the steps that a 50 steel plate with the thickness h smaller than or equal to 20 mm is placed on a straightening machine to be straightened, and straightening parameters include the straightening starting temperature of the 50 steel plate ranging from 820 DEG C to 890 DEG C, the total rolling reduction of straightening ranging from 0.8 mm to 1.2 mm and the cooling bed feeding temperature smaller than or equal to 670 DEG C. And the 50 steel plate is prevented from being bent by controlling parameters in the straightening process. By reducing the initial straightening temperature of the 50 steel plate, reducing the deformation stress of the 50 steel plate and cooperatively increasing the total rolling reduction of the 50 steel plate, the head end and the tail end of the 50 steel plate can be effectively prevented from being bent. The temperature of the 50 steel plate on the cooling bed is further reduced, the influence of abrasion generated after the cooling bed is used for a long time on the shape of the 50 steel plate is avoided, and the bending possibility of the 50 steel plate is further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel production, and in particular to a straightening method for thin-gauge 50 steel and application thereof. Background Art

[0002] 50 steel is a kind of high-quality carbon structural steel plate. It contains less sulfur, phosphorus and non-metallic inclusions and has excellent mechanical properties. Therefore, it is widely used in the manufacture of general structures and mechanical structure parts, building structures, pipes for conveying fluids and plastic molds.

[0003] 50 steel is generally produced in plate form. When rolling thin (16-20mm) 50 steel plates in the special rolling mill, the temperature or cooling rate of the steel plates is inconsistent, resulting in bending of the steel plates after the cooling bed. Among all the bending types of 50 steel, transverse bending and longitudinal bending are the main ones, and the bending mainly occurs in the head plate and the tail plate. Therefore, ensuring the controllable plate quality of the head plate and the tail plate is of great significance for the production of 50 steel. When 50 steel has transverse and / or longitudinal bending, the steel plate cannot be directly put into storage, and needs to be re-entered into the heat treatment furnace for normalizing treatment to eliminate the organizational stress and ensure the flatness of the plate surface, which undoubtedly increases the post-processing cost and reduces production efficiency.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a straightening method for thin gauge 50 steel and application thereof.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a method for straightening thin-gauge 50 steel, comprising placing a 50 steel plate with a thickness of h≤20 mm on a straightening machine for straightening.

[0008] The straightening parameters include: the starting straightening temperature of 50 steel plate is 820~890℃, the total straightening reduction is 0.8~1.2mm, and the upper cooling bed temperature is ≤670℃.

[0009] In an optional embodiment, the tilt value of the straightening machine is 1.4-1.6 mm.

[0010] In an optional embodiment, when the thickness h of the 50 steel plate is less than 18 mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 830-890°C, the total straightening reduction is 0.9-1.1 mm, and the upper cooling bed temperature is ≤650°C.

[0011] In an optional embodiment, when the thickness of the 50 steel plate is 18mm≤h<19mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 820-880°C, the total straightening reduction is 0.8-1.2mm, and the upper cooling bed temperature is ≤650°C.

[0012] In an optional embodiment, when the thickness of the 50 steel plate is 19mm≤h≤20mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 820-880°C, the total straightening reduction is 0.8-1.2mm, and the upper cooling bed temperature is ≤670°C.

[0013] In an optional embodiment, the rotation speed of the roller conveying the 50 steel plates is 85-95 revolutions per minute, and the straightening pressure of the 50 steel plates is 1800-2200 Newtons.

[0014] In an optional embodiment, the straightening process of the 50 steel plate includes two straightening passes at 6 to 8 mm on both ends of the 50 steel plate.

[0015] In an optional embodiment, the straightening process of the 50 steel plate further includes performing a straightening pass in the middle section of the 50 steel plate.

[0016] In an optional embodiment, cooling water is not turned on outside the straightening rollers before, during and after straightening.

[0017] In a second aspect, the present invention provides an application of a straightening method according to any one of the aforementioned embodiments in reducing bending of thin-gauge 50 steel during the production process.

[0018] The present invention has the following beneficial effects:

[0019] The present invention provides a straightening method for thin-gauge 50 steel and its application, which can prevent the 50 steel plate from bending by controlling the parameters of the straightening process. By lowering the start straightening temperature of the 50 steel plate, reducing the deformation stress of the 50 steel plate, and increasing the total reduction of the 50 steel plate, the bending of the head and tail ends of the 50 steel plate can be effectively prevented. Further lowering the upper cooling bed temperature of the 50 steel plate can prevent the wear of the cooling bed after long-term use from affecting the shape of the 50 steel, and further reduce the possibility of bending of the 50 steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0021] Figure 150 steel for producing transverse bending provided in Test Example 1 of the present invention;

[0022] Figure 2 50 steel for producing longitudinal bending provided in Test Example 1 of the present invention;

[0023] Figure 3 The 50 steel with turtle back bending provided in Test Example 1 of the present invention;

[0024] Figure 4 The 50 steel that produces edge wave bending is provided in Test Example 1 of the present invention. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0026] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0027] In a first aspect, the present invention provides a method for straightening thin-gauge 50 steel, comprising placing a 50 steel plate with a thickness of h≤20 mm on a straightening machine for straightening.

[0028] The straightening parameters include: the starting straightening temperature of 50 steel plate is 820~890℃, the total straightening reduction is 0.8~1.2mm, and the upper cooling bed temperature is ≤670℃.

[0029] For example, the start-leveling temperature of the 50 steel plate can be any value among 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C or 890°C, or a range between any two values, or any point in the above range. Preferably, the start-leveling temperature of the 50 steel plate is 850-860°C.

[0030] For example, the total straightening reduction is any value among 0.8mm, 0.9mm, 1.0mm, 1.1mm or 1.2mm, or a range between any two values, or any point in the above range. Preferably, the total straightening reduction is 1.0mm.

[0031] For example, the upper cooling bed temperature is any value among 670°C, 660°C, 650°C, 640°C, 630°C or 620°C, or a range value between any two values, or any point value in the above range values.

[0032] By controlling the parameters of the straightening process, the bending of the 50 steel plate can be avoided. By lowering the start straightening temperature of the 50 steel plate, reducing the deformation stress of the 50 steel plate, and increasing the total reduction of the 50 steel plate, the bending of the 50 steel plate at both ends can be effectively prevented. Further reducing the temperature of the upper cooling bed of the 50 steel plate can prevent the wear of the cooling bed after long-term use from affecting the shape of the 50 steel, further reducing the possibility of bending of the 50 steel.

[0033] In an optional embodiment, the tilting value of the straightener is 1.4-1.6 mm. For example, it can be any value among 1.4 mm, 1.5 mm or 1.6 mm, or a range value between any two values, or any point value in the above range value. Preferably, the tilting value of the straightener is 1.5 mm.

[0034] By controlling the tilt value within the above range, the bend of the 50 steel plate can be effectively straightened and the straightening effect can be improved.

[0035] In an optional embodiment, when the thickness h of the 50 steel plate is less than 18 mm, for example, when the thickness h of the 50 steel plate is 16 mm or 17 mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 830-890°C, the total straightening reduction is 0.9-1.1 mm, and the upper cooling bed temperature is ≤650°C.

[0036] Preferably, when the thickness h of the 50 steel plate is less than 18 mm, for example, when the thickness h of the 50 steel plate is 16 mm or 17 mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 860°C, the total straightening reduction is 1.0 mm, and the upper cooling bed temperature is ≤650°C.

[0037] In an optional embodiment, when the thickness of the 50 steel plate is 18mm≤h<19mm, for example, when the thickness h of the 50 steel plate is 18mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 820-880°C, the total straightening reduction is 0.8-1.2mm, and the upper cooling bed temperature is ≤650°C.

[0038] Preferably, when the thickness of the 50 steel plate is 18mm≤h<19mm, for example, when the thickness h of the 50 steel plate is 18mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 850℃, the total straightening reduction is 1.0mm, and the upper cooling bed temperature is ≤650℃.

[0039] In an optional embodiment, when the thickness of the 50 steel plate is 19mm≤h≤20mm, for example, when the thickness h of the 50 steel plate is 19mm or 20mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 820-880°C, the total straightening reduction is 0.8-1.2mm, and the upper cooling bed temperature is ≤670°C.

[0040] Preferably, when the thickness of the 50 steel plate is 19mm≤h≤20mm, for example, when the thickness h of the 50 steel plate is 19mm or 20mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 850℃, the total straightening reduction is 1.0mm, and the upper cooling bed temperature is ≤670℃.

[0041] The parameters of the straightening process are adjusted according to the thickness of the 50 steel plate. When the thickness of the 50 steel plate is small, the straightening temperature is relatively high, which can ensure the smooth progress of the straightening process; when the thickness of the 50 steel plate is large, the straightening temperature is relatively low to prevent the bending phenomenon caused by uneven temperature in different parts of the 50 steel plate.

[0042] When the thickness of the 50 steel plate is small, reduce the total straightening reduction to prevent bending caused by over-straightening; when the thickness of the 50 steel plate is large, increase the total straightening reduction appropriately to reduce the bending of the 50 steel plate.

[0043] When the thickness of the 50 steel plate is small, the temperature of the upper cooling bed is lowered to prevent the wear and tear caused by long-term use of the cooling bed from affecting the shape of the steel plate; when the thickness of the 50 steel plate is large, the temperature of the upper cooling bed can be appropriately increased to reduce energy consumption. Because when the thickness of the steel plate is large, the wear and tear on the cooling bed has a relatively small effect on the shape of the steel plate, and it is not easy to cause the steel plate to bend.

[0044] In an optional embodiment, during the straightening process, the rotation speed of the roller conveying the 50 steel plates is 85-95 revolutions per minute, and the straightening pressure of the 50 steel plates is 1800-2200 Newtons.

[0045] In an optional embodiment, the straightening process of the 50 steel plate includes two straightening passes at 6 to 8 mm on both ends of the 50 steel plate.

[0046] Since the head and tail ends of the 50 steel plate are most prone to bending, during the straightening process, the straightening times can be increased for the locations prone to bending. However, the selection of the length of the area where the straightening times are increased has a significant impact on the straightening effect. When the length of the area where the straightening times are increased is too long, the stress of the 50 steel plate may increase and bend; when the length of the area where the straightening times are increased is too short, the straightening length of the 50 steel plate may be insufficient and bend. The present invention controls the length of the area where the straightening times are increased within 6 to 8 mm, which can effectively reduce the occurrence of bending of the 50 steel plate.

[0047] In an optional embodiment, the straightening process of the 50 steel plate further includes straightening once in the middle section of the 50 steel plate. That is, after straightening twice the 5-8 mm area at the head end of the 50 steel plate, the 50 steel plate is passed through the straightening machine as a whole for straightening once, and then straightened twice at the 5-8 mm area at the tail end of the 50 steel plate to complete the straightening process.

[0048] In an optional embodiment, cooling water is not turned on outside the straightening rollers during the entire straightening process, e.g. before, during and after straightening, to avoid water on the surface of the 50 steel plate during the straightening process, which would affect the surface quality of the 50 steel plate.

[0049] In a second aspect, the present invention provides an application of a straightening method according to any one of the aforementioned embodiments in reducing bending of thin-gauge 50 steel during the production process.

[0050] Example 1

[0051] This embodiment provides a straightening method for thin-gauge 50 steel, wherein the 50 steel provided in this embodiment is in plate shape with a thickness of 16 mm. The specific steps are as follows:

[0052] The 50 steel plate obtained by rolling is sent to the straightening machine, and two straightening passes are performed at 6 to 8 mm at the head and tail ends of the 50 steel plate, and one straightening pass is performed in the middle section.

[0053] Do not open the cooling water outside the straightening rollers before, during and after straightening to avoid water on the surface of the 50 steel plate during the straightening process, which will affect the surface quality of the 50 steel plate.

[0054] The straightening parameters include: the starting straightening temperature of the 50 steel plate is 883℃, the tilting value is 1.5mm, the speed of the roller conveying the 50 steel plate is 90 rpm, the straightening pressure is 2000N, the total straightening reduction is 1.0mm±0.1mm, and the upper cooling bed temperature is 643℃.

[0055] Example 2

[0056] This embodiment provides a straightening method for thin-gauge 50 steel, wherein the 50 steel provided in this embodiment is in plate shape with a thickness of 17 mm. The specific steps are as follows:

[0057] The 50 steel plate obtained by rolling is sent to the straightening machine, and two straightening passes are performed at 6 to 8 mm at the head and tail ends of the 50 steel plate, and one straightening pass is performed in the middle section.

[0058] Do not open the cooling water outside the straightening rollers before, during and after straightening to avoid water on the surface of the 50 steel plate during the straightening process, which will affect the surface quality of the 50 steel plate.

[0059] The straightening parameters include: the starting straightening temperature of the 50 steel plate is 873℃, the tilting value is 1.5mm, the speed of the roller conveying the 50 steel plate is 90 rpm, the straightening pressure is 2000N, the total straightening reduction is 1.0mm±0.1mm, and the upper cooling bed temperature is 637℃.

[0060] Example 3

[0061] This embodiment provides a straightening method for thin-gauge 50 steel, wherein the 50 steel provided in this embodiment is in plate shape with a thickness of 18 mm. The specific steps are as follows:

[0062] The 50 steel plate obtained by rolling is sent to the straightening machine, and two straightening passes are performed at 6 to 8 mm at the head and tail ends of the 50 steel plate, and one straightening pass is performed in the middle section.

[0063] Do not open the cooling water outside the straightening rollers before, during and after straightening to avoid water on the surface of the 50 steel plate during the straightening process, which will affect the surface quality of the 50 steel plate.

[0064] The straightening parameters include: the starting straightening temperature of the 50 steel plate is 867℃, the tilting value is 1.5mm, the speed of the roller conveying the 50 steel plate is 90 rpm, the straightening pressure is 2000N, the total straightening reduction is 1.0mm±0.2mm, and the upper cooling bed temperature is 636℃.

[0065] Example 4

[0066] This embodiment provides a straightening method for thin-gauge 50 steel, wherein the 50 steel provided in this embodiment is in plate shape with a thickness of 19 mm. The specific steps are as follows:

[0067] The 50 steel plate obtained by rolling is sent to the straightening machine, and two straightening passes are performed at 6 to 8 mm at the head and tail ends of the 50 steel plate, and one straightening pass is performed in the middle section.

[0068] Do not open the cooling water outside the straightening rollers before, during and after straightening to avoid water on the surface of the 50 steel plate during the straightening process, which will affect the surface quality of the 50 steel plate.

[0069] The straightening parameters include: the starting straightening temperature of the 50 steel plate is 871°C, the tilting value is 1.5mm, the speed of the roller conveying the 50 steel plate is 90 rpm, the straightening pressure is 2000N, the total straightening reduction is 1.0mm±0.2mm, and the upper cooling bed temperature is 657°C.

[0070] Example 5

[0071] This embodiment provides a straightening method for thin-gauge 50 steel, wherein the 50 steel provided in this embodiment is in plate shape with a thickness of 20 mm. The specific steps are as follows:

[0072] The 50 steel plate obtained by rolling is sent to the straightening machine, and two straightening passes are performed at 6 to 8 mm at the head and tail ends of the 50 steel plate, and one straightening pass is performed in the middle section.

[0073] Do not open the cooling water outside the straightening rollers before, during and after straightening to avoid water on the surface of the 50 steel plate during the straightening process, which will affect the surface quality of the 50 steel plate.

[0074] The straightening parameters include: the starting straightening temperature of the 50 steel plate is 862℃, the tilting value is 1.5mm, the speed of the roller conveying the 50 steel plate is 90 rpm, the straightening pressure is 2000N, the total straightening reduction is 1.0mm±0.2mm, and the upper cooling bed temperature is 661℃.

[0075] Comparative Example 1

[0076] This comparative example provides a straightening method for thin-gauge 50 steel, which is applicable to 50 steel plates with a thickness of 16 to 20 mm. The specific steps are as follows:

[0077] The 50 steel plate obtained by rolling is sent to the straightening machine, and two to three straightening passes are performed at 8 to 10 mm at the head and tail ends of the 50 steel plate, and one straightening pass is performed in the middle section.

[0078] The cooling water outside the straightening rollers is not turned on before and during straightening. After straightening, the cooling water outside the straightening rollers is turned on to cool down the 50 steel plate.

[0079] The straightening parameters include: the starting straightening temperature of 50 steel plate is 900℃~930℃, the tilting value is 1.5mm, the speed of the roller conveying 50 steel plate is 90 rpm, the straightening pressure is 2000N, the total straightening reduction is 0mm~0.5mm, and the upper cooling bed temperature is 680~700℃.

[0080] Comparative Example 2

[0081] This comparative example provides a straightening method for thin-gauge 50 steel, and the specific steps are similar to those of Examples 1 to 5, with the only difference being that the total straightening reduction of the 50 steel is 0.5 to 1.0 mm.

[0082] Comparative Example 3

[0083] This comparative example provides a straightening method for thin-gauge 50 steel, and the specific steps are similar to those of Examples 1 to 5, with the only difference being that the temperature of the upper cooling bed changes to 700° C. to 750° C. after the 50 steel is straightened.

[0084] Test Example 1

[0085] The 50 steels obtained by the straightening methods provided in Examples 1 to 5 and Comparative Examples 1 to 3 were tested, wherein the straightening method of each embodiment produced 50 steels, and the bending conditions of the 50 steels obtained by each method were calculated, and the bending conditions of the 50 steels obtained by each method were obtained as shown in Tables 1 and Figure 1 to Figure 4 Results shown.

[0086] Table 1 Bending of 50 steel

[0087]

[0088] The "other" in Table 1 refers to other bending conditions besides transverse bending and longitudinal bending, such as turtle back bending or side wave bending, etc. Figure 1 to Figure 4 .

[0089] As can be seen from Table 1, the embodiment of the present invention provides a straightening method for thin-gauge 50 steel. After straightening, the number of bending cases of the 50 steel is the least and the bending rate is low, which avoids the situation where the 50 steel needs to be reworked and post-processed after bending, thereby improving the production efficiency and stability of the production quality of the 50 steel.

[0090] Comparative Example 1 adopts the existing straightening method, the start straightening temperature is high, and the upper cooling bed temperature is high, which makes the 50 steel plate easy to deform, resulting in an increase in curvature. Comparative Example 2 increases the total reduction in the straightening process, which may cause excessive straightening and deformation, so the deformation rate of Comparative Example 2 is also increased compared with the embodiment. Comparative Example 3 changes the upper cooling bed temperature, which also causes the 50 steel temperature to be too high and easy to deform, and the curvature is increased compared with the embodiment.

[0091] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for straightening thin gauge 50 steel, It is characterized in that It includes placing a 50 steel plate with a thickness of h≤20mm on a straightening machine for straightening; The straightening parameters include: the starting straightening temperature of the 50 steel plate is 820-890°C, the total straightening reduction is 0.8-1.2 mm, and the upper cooling bed temperature is ≤670°C.

2. The straightening method according to claim 1, It is characterized in that The tilting value of the straightening machine is 1.4 to 1.6 mm.

3. The straightening method according to claim 2, It is characterized in that When the thickness h of the 50 steel plate is less than 18 mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 830-890° C., the total straightening reduction is 0.9-1.1 mm, and the upper cooling bed temperature is ≤650° C.

4. The straightening method according to claim 2, It is characterized in that When the thickness of the 50 steel plate is 18mm≤h<19mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 820-880°C, the total straightening reduction is 0.8-1.2mm, and the upper cooling bed temperature is ≤650°C.

5. The straightening method according to claim 2, It is characterized in that When the thickness of the 50 steel plate is 19mm≤h≤20mm, the straightening parameters include: the starting straightening temperature of the 50 steel plate is 820-880°C, the total straightening reduction is 0.8-1.2mm, and the upper cooling bed temperature is ≤670°C.

6. The straightening method according to any one of claims 3 to 5, It is characterized in that The rotation speed of the roller conveying the 50 steel plate is 85-95 revolutions / min, and the straightening pressure of the 50 steel plate is 1800-2200N.

7. The straightening method according to any one of claims 3 to 5, It is characterized in that The straightening process of the 50 steel plate includes two straightening passes at 6 to 8 mm at both ends of the 50 steel plate.

8. The straightening method according to claim 7, It is characterized in that The straightening process of the 50 steel plates also includes performing a straightening pass in the middle section of the 50 steel plates.

9. The straightening method according to claim 1, It is characterized in that Do not turn on cooling water outside the straightening rollers before, during and after straightening.

10. Use of the straightening method according to any one of claims 1 to 9 in reducing the bending of thin-gauge 50 steel during the production process.

Citation Information

Patent Citations

  • Production method of controlling pattern block of normalizing thin gauge steel plate

    CN106734317A

  • Method for controlling transverse unevenness of hot-rolled steel plate with thickness specification smaller than or equal to 50 mm

    CN114433638A

  • Energy-saving and consumption-reducing manufacturing method for producing steel plate with thin specification of 6 mm through wide and thick plate rolling mill

    CN116493412A

  • Facility for producing hot-rolled steel plate, and its production method

    JP2005074480A