Copper-chromium alloy and preparation method and application thereof
By adjusting the composition and process of copper-chromium alloy raw materials, the problem of insufficient performance of copper materials in the MIM process is solved, the thermal conductivity and hardness are improved, the demand for 1600G signal optical communication is met, and the field of optical communication is provided with high Properties material.
Patent Information
- Application Number
- CN202411185923.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The copper feeding of the existing MIM process is not ideal, resulting in insufficient product performance, especially in terms of thermal conductivity and hardness, which cannot meet the needs of 1600G signal optical communication.
By adjusting the composition of the copper-chromium alloy raw material, the Cr content is increased by 0.5-1.5% and the Zr content is 0.05-0.25%, and the Ag element is added, combined with appropriate MIM process and acid-catalyzed degreasing treatment, the thermal conductivity and hardness of the material are improved, ensuring that The thermal conductivity is between 370-390W·M-1·K-1 and hardness HV≥110, and the conductivity is increased to ≥59.6×106S/m.
It has achieved the performance improvement of copper-chromium alloy, meets the thermal conductivity, hardness and conductivity requirements in the field of optical communication, and has good processing performance and environmental protection, and is suitable for high-performance materials in the field of optical communication.
Smart Images

Figure CN119057060A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical communication metal materials, and in particular relates to a copper-chromium alloy and a preparation method and application thereof. Background Art
[0002] With the rapid development of the AI era, the demand for high-speed and large-capacity signal transmission in the 5G communication field is growing. 800G signal optical communication has gradually failed to meet the needs of the times, and the transition of signal optical communication to 1600G has become an inevitable trend. However, the existing zinc-aluminum alloy material is not ideal in terms of heat dissipation, which has become one of the key factors restricting the further development of optical communication technology.
[0003] Copper materials have become a potential alternative to zinc-aluminum alloys due to their excellent thermal conductivity. However, the traditional manufacturing process of copper products has many shortcomings, such as high material waste, large processing volume, and high processing costs. Therefore, the development of new manufacturing processes, especially MIM processes, is of great significance for improving the performance and reducing costs of copper products. However, the copper feed suitable for MIM process on the market is not ideal, and the performance of processed products often does not meet the use requirements. This is mainly reflected in the product's variability and insufficient thermal conductivity. Variability may cause the product to change shape or deteriorate in performance during use, which directly affects the signal transmission efficiency and stability of optical communication equipment.
[0004] At present, the market lacks MIM copper preparation processes and supporting raw materials and products that can meet industrial performance requirements. Summary of the invention
[0005] The technical problem to be solved by the present invention is that the feeding of the existing MIM process is not ideal and the product performance is insufficient. The shortcomings and defects mentioned in the above background technology are overcome and a copper-chromium alloy and a preparation method and application thereof are provided.
[0006] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0007] A copper-chromium alloy, wherein the raw materials of the copper-chromium alloy include a metal raw material and a binder, and the volume ratio of the binder to the metal is 11:100;
[0008] The metal raw materials include the following components according to weight:
[0009] Si content is 0.18-0.22%, Cu content is 98.5-99.5%, Fe content is 0.01-0.03%, Ni content is 0.02-0.04%, Cr content is 0.5-1.5%, Zr content is 0.05-0.25%, and Ag content is 0.3-0.5%.
[0010] Traditional copper-chromium alloy materials mostly contain elements Si, Cu, Fe, and Ni. The heat dissipation and electrical conductivity of the products produced are insufficient and cannot meet the requirements of 1600G products. In view of the above problems, the present invention adds 0.5-1.5% Cr to the copper-chromium alloy raw material to increase the thermal conductivity of the material, and adds 0.05-0.25% Zr to increase the hardness of the material. The addition of these two elements significantly improves the thermal conductivity and hardness of the material, so that it can meet the thermal conductivity (370-390) W·M -1 ·K -1 and hardness HV ≥ 110; secondly, in order to improve the conductivity of the material, we added Ag element, the content of which was controlled at 0.3-0.5%. Ag is an excellent conductive material, and its addition makes the conductivity of the copper-chromium alloy reach ≥ 59.6×10 6 S / m requirements.
[0011] Preferably, the binder is a plastic-based binder, which comprises 65% by mass of polystyrene, 16% by mass of polyethylene, 12% by mass of stearic acid and 10% by mass of diethyl phthalate.
[0012] Plastic-based binders are degreased quickly by acid catalysis, and the by-products are all CO 2 、N 2 It is a safe gas with simple equipment and easy management. At the same time, the wax-based binder has a short sintering time and the product has little deformation.
[0013] Preferably, the thermal conductivity of the copper-chromium alloy is 370-390 W·M -1 ·K -1 , hardness HV ≥ 110, conductivity ≥ 59.6 × 10 6 S / m.
[0014] Based on a general inventive concept, the present invention also provides a method for preparing the copper-chromium alloy, comprising the following steps:
[0015] (1) preparing ingredients according to the raw materials of the copper-chromium alloy, and mixing them by banburying to obtain a mixed material;
[0016] (2) injection molding the mixed material to obtain an alloy green body;
[0017] (3) The alloy green body is subjected to an acid-catalyzed degreasing treatment to obtain a copper-chromium alloy.
[0018] Preferably, the mixing temperature is 180-200° C., and the granulation time is 6-7 h.
[0019] Preferably, the injection molding parameters include: injection speed of 100±30% mm / s, injection pressure of 195±30% MPa, screw forward position of 10±10 mm, holding pressure of 70±30% MPa, time of 40±1s, mold opening and closing speed of 30% mm / s, mold opening and closing pressure of 40±30% MPa, and mold opening position of 10±10 mm.
[0020] Preferably, the screw switching position of the injection molding is 10±15.0 mm, and the metering residual material amount is 5±5.0 mm.
[0021] Preferably, the injection molding cycle is 10-20s, the cooling time is 1-11s, and the cycle time difference between using a robot and not using a robot is 5-15s.
[0022] Preferably, the acid-catalyzed degreasing treatment is high-temperature combustion after acid catalysis, the high temperature is 900-1000 degrees Celsius, and the acids used include 30g / L-50g / L sulfuric acid, 3g / L-8g / L ammonium bifluoride, 2g / L-4g / L citric acid, 1g / L-3g / L sodium nitrate, 0.5g / L-1.5g / L ferric sulfate or 1g / L-2g / L dipropylene glycol. Among them, sulfuric acid can be used as an auxiliary component to synergize with other acids to improve the degreasing effect and help enhance the permeability and solubility of the degreasing agent; citric acid mainly plays a corrosion inhibition role in the acidic degreasing solution, which can effectively inhibit the corrosion of metals such as copper in acidic media; sodium nitrate mainly plays an oxidative fluxing role. Ammonium bifluoride has strong corrosiveness and solubility, and can react with grease, dirt and oxides on the metal surface to achieve a decontamination effect.
[0023] The above acids have a fast catalytic degreasing speed, and the by-products are all CO 2 、N 2 The safety index is high and it is environmentally friendly. Through degreasing treatment, impurities and excess components in the material can be effectively removed, further improving the performance of the material.
[0024] Based on a general inventive concept, the present invention also provides an application of the copper-chromium alloy, and the copper-chromium alloy is used in the field of optical communications.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention provides a copper-chromium alloy to solve the problems of processing deformation and insufficient thermal conductivity of copper-chromium alloy feed in MIM process. The thermal conductivity of copper-chromium alloy is 370-390 W·M -1 ·K -1 , hardness HV ≥ 110, conductivity ≥ 59.6 × 10 6S / m, which can meet the performance requirements in the field of optical communications; copper-chromium alloy materials not only have excellent thermal conductivity, hardness and electrical conductivity, but also have good processing performance and environmental protection, and are expected to be widely used in optical communications and other fields;
[0027] (2) The preparation method of the copper-chromium alloy of the present invention optimizes the ratio of the copper-chromium alloy, adjusts the element content in the ingredients, and uses an appropriate MIM process to successfully improve the thermal conductivity and hardness of the material so that it meets specific performance requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a specific picture of the copper-chromium alloy obtained in Example 1 being applied in the field of optical communications and used in optical communications accessories. DETAILED DESCRIPTION
[0030] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0031] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0032] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0033] Example 1
[0034] This embodiment provides a copper-chromium alloy, wherein the raw materials of the copper-chromium alloy include a metal raw material and a binder, and the volume ratio of the binder to the metal is 11:100;
[0035] The metal raw materials are counted by weight and include the following components:
[0036] Si content is 1.8g, Cu content is 985g, Fe content is 0.1g, Ni content is 0.2g, Cr content is 5g, Zr content is 5g, and Ag content is 3g.
[0037] The binder is 650g polystyrene, 160g polyethylene, 120g stearic acid and 100g diethyl phthalate in parts by mass.
[0038] The method for preparing the copper-chromium alloy of this embodiment comprises the following steps:
[0039] (1) According to the raw materials of the copper-chromium alloy, the raw materials are first added, the metal raw materials are mixed evenly, and then the binder is added, and the mixture is kneaded and granulated at 180 degrees Celsius to obtain a mixture, and the granulation time is 6-7 hours;
[0040] (2) The process parameters of injection molding are set as follows: injection speed 100 mm / s, injection pressure 195 MPa, screw forward position 10 mm, holding pressure 70 MPa, time 40 s, mold opening and closing speed 30% mm / s, mold opening and closing pressure 40% MPa, mold opening position 10 mm; screw switching position 10 mm, metering residual material 5 mm; injection molding cycle 15 s, cooling time 6 s, and the cycle time difference between using a robot and not using a robot is 10 s;
[0041] Starting the molding equipment to injection mold the mixed material to obtain an alloy green body;
[0042] (3) The alloy green body is acid-catalyzed and then burned at high temperature, the high temperature is 900-1000 degrees Celsius, and the acid used is a mixed acid of 30g / L-50g / L sulfuric acid, 3g / L-8g / L ammonium bifluoride, 2g / L-4g / L citric acid, 1g / L-3g / L sodium nitrate, 0.5g / L-1.5g / L ferric sulfate, and 1g / L-2g / L dipropylene glycol to obtain a copper-chromium alloy.
[0043] The obtained copper-chromium alloy was subjected to product performance tests:
[0044] 1. Thermal conductivity determination, the test method is GB / T 22588-2008, prepare the thermal conductivity determination instrument, turn on the instrument, put in the test piece to be measured, click to start the test, the test time is 3h, and wait for the data output;
[0045] 2. Hardness and conductivity test
[0046] Environmental conditions Temperature: 23±2℃; Humidity: 50±5%RH Test standard: ASTM E1269-11 (Reapproved2018), GB / T 1423-1996, GB / T 22588-2008 Test conditions Test model: Cowan model + pulse correction;
[0047] The test results are shown in Table 1 below. The thermal conductivity of the copper-chromium alloy obtained in this embodiment is 370-390 W·M -1 ·K-1 , hardness HV ≥ 110, conductivity ≥ 59.6 × 10 6 S / m.
[0048] Table 1 Performance test results of copper-chromium alloy products of Example 1 and Comparative Examples 1-3
[0049]
[0050] The copper-chromium alloy of this embodiment is applied to optical communication accessories in the field of optical communication. Figure 1 As shown, the durability of the product is improved and the waste after processing can be easily recycled.
[0051] Comparative Example 1:
[0052] The rest of this comparative example is exactly the same as Example 1, with the only difference being that the metal raw material does not contain Cr, Zr and Ag.
[0053] Comparative Example 2:
[0054] The rest of this comparative example is exactly the same as Example 1, with the only difference being that the metal raw material does not contain Zr and Ag.
[0055] Comparative Example 3:
[0056] The rest of this comparative example is exactly the same as Example 1, with the only difference being that the metal raw material does not contain Ag.
Claims
1. A copper-chromium alloy, characterized in that: The raw materials of the copper-chromium alloy include a metal raw material and a binder, and the volume ratio of the binder to the metal is 105-115:995-1005; The metal raw materials include the following components according to weight: Si content is 0.18-0.22%, Cu content is 98.5-99.5%, Fe content is 0.01-0.03%, Ni content is 0.02-0.04%, Cr content is 0.5-1.5%, Zr content is 0.05-0.25%, and Ag content is 0.3-0.5%.
2. The alloy according to claim 1, characterized in that The adhesive is a plastic-based adhesive, which includes 60-65% by mass of polystyrene, 16-20% by mass of polyethylene, 12-15% by mass of stearic acid and 10-15% by mass of diethyl phthalate.
3. The alloy according to claim 1, characterized in that The thermal conductivity of the copper-chromium alloy is 370-390 W·M -1 ·K -1 , hardness HV ≥ 110, conductivity ≥ 59.6 × 10 6 S / m.
4. A method for preparing the copper-chromium alloy according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) preparing ingredients according to the raw materials of the copper-chromium alloy, mixing and granulating to obtain a mixed material; (2) injection molding the mixed material to obtain an alloy green body; (3) The alloy green body is subjected to an acid-catalyzed degreasing treatment to obtain a copper-chromium alloy.
5. The preparation method according to claim 1, characterized in that: The mixing temperature is 180-200° C., and the granulation time is 6-7 hours.
6. The preparation method according to claim 1, characterized in that: The injection molding parameters include: injection speed of 100±30% mm / s, injection pressure of 195±30% MPa, screw forward position of 10±10 mm, holding pressure of 70±30% MPa, time of 40±1s, mold opening and closing speed of 30% mm / s, mold opening and closing pressure of 40±30% MPa, and mold opening position of 10±10 mm.
7. The preparation method according to claim 1, characterized in that: The screw switching position of the injection molding is 10±15.0 mm, and the metering residual material is 5±5.0 mm.
8. The preparation method according to claim 1, characterized in that: The injection molding cycle is 10-20 seconds, the cooling time is 1-11 seconds, and the cycle time difference between using a robot and not using a robot is 5-15 seconds.
9. The preparation method according to claim 1, characterized in that: The acid-catalyzed degreasing treatment is acid-catalyzed followed by high-temperature combustion, the high temperature being 900-1000 degrees Celsius, and the acids used include 30g / L-50g / L sulfuric acid, 3g / L-8g / L ammonium bifluoride, 2g / L-4g / L citric acid, 1g / L-3g / L sodium nitrate, 0.5g / L-1.5g / L ferric sulfate or 1g / L-2g / L dipropylene glycol.
10. An application of the copper-chromium alloy according to any one of claims 1 to 3, characterized in that: The copper-chromium alloy is used in the field of optical communication.
Citation Information
Patent Citations
Chrome zirconium copper alloy and preparing and processing method thereof
CN101717876A
High-strength high-conductivity copper-chromium-zirconium alloy and preparation method thereof
CN109112347A
Low-beryllium multi-component copper alloy for crystallizer and preparation method thereof
CN116287848A
High-strength and high-conductivity copper alloy plate strip and preparation method thereof
CN116623071A
Copper alloy sheet material and method for producing same
US20180274074A1