Honeycomb sandwich structure thermal insulation material and preparation method thereof

By adding low-density inorganic filler and film structure to the anti-insulation material of honeycomb sandwich structure, the existing anti-insulation materials have solved the problem of insufficient temperature resistance and low strength in high-temperature environments, and the efficient insulation of high-speed aircraft is achieved. Improved mechanical properties.

CN119058213APending Publication Date: 2024-12-03BEIJING COMPOSITE MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411374454.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing anti-insulation materials are insufficient in temperature resistant, have low strength and are easy to destroy in high-temperature environments, making it difficult to meet the anti-insulation needs of high-speed aircraft.

Method used

Using honeycomb sandwich structure anti-insulating material, the honeycomb core material and skin layer are arranged by alternately laminating, and low-density inorganic fillers such as hollow glass microbeads or silica aerogel powder are added to the polyimide matrix to combine with the glue film Structure, improve the insulation, insulation and mechanical properties of the material.

Benefits of technology

It has achieved good thermal insulation performance and lightweight and high-strength anti-insulating materials at high temperatures above 600℃, which are suitable for external protection of high-speed aircraft.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005068348170000111
    Figure BDA0005068348170000111
Patent Text Reader

Abstract

The invention provides a honeycomb sandwich structure heat prevention and insulation material and a preparation method thereof, and the honeycomb sandwich structure heat prevention and insulation material comprises a honeycomb core material and a skin layer which are alternately stacked; an adhesive film is arranged between the honeycomb core material and the skin layer; the honeycomb core material comprises a paper honeycomb core strip and phthalonitrile resin; the phthalonitrile resin is compounded on the surface and inside the paper honeycomb core strip; the skin layer is prepared from a reinforcing material and a resin solution; the resin solution comprises a polyimide resin solution and an inorganic filler. The honeycomb sandwich structure heat-proof and heat-insulating material prepared by the method can resist the temperature of 600 DEG C or above, and can be used as a high-temperature-resistant heat-proof and heat-insulating material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of heat-insulating materials, and in particular relates to a honeycomb sandwich structure heat-insulating material and a preparation method thereof. Background Art

[0002] As the speed of aircraft continues to increase, the requirements for high temperature resistance, mechanical properties and light weight of aircraft materials are getting higher and higher. When high-speed aircraft fly in the atmosphere, the shell is subjected to complex and severe mechanical and thermal conditions in the aerodynamic environment. In order to prevent high temperature from damaging the internal equipment, the shell must be covered with materials with good heat insulation performance to protect it.

[0003] Heat-proof materials are usually composed of high-density fiber reinforcement and resin composites, and most of the heat is taken away by melt sublimation under high airflow. At present, the most commonly used insulation materials are resin-based foam materials, ceramic insulation tiles and aerogel composite materials. However, they all have certain disadvantages. Traditional resin-based foam materials have excellent thermal insulation properties, but their temperature resistance is generally low and it is difficult to meet the use requirements. Ceramic rigid insulation tiles have excellent thermal insulation properties, but their strength is low and their toughness is poor. They are prone to brittle failure during production, transportation or use, and there are great safety hazards; aerogel composite materials have good thermal insulation properties, and inorganic aerogels can withstand temperatures of more than 600°C, but aerogels have poor strength and are difficult to withstand external forces and scouring, so they cannot be used as outer insulation materials.

[0004] For example, a Chinese patent document with publication number CN114349490B discloses a silica aerogel insulation material and a preparation method thereof, wherein the silica aerogel insulation material is prepared by gel injection molding, and the raw materials for preparing the silica aerogel insulation material include silica aerogel, infrared sunscreen and gel injection molding raw materials. The silica aerogel insulation material prepared by the invention can be used for a long time in an environment where insulation is required and subjected to rapid cooling and heating. At the same time, the silica aerogel insulation material prepared by the method increases the maximum use temperature from the traditional 650°C to 800°C without adding other substances such as alumina aerogel or refractory fiber, greatly broadening the scope of application of silica aerogel. Moreover, after sintering, a sample of a predetermined size of ordinary shape or special complex shape can be obtained without processing or minor processing. However, the silica aerogel insulation material prepared by this method has poor strength and is difficult to withstand external forces and scouring.

[0005] Therefore, it is necessary to study a material with excellent heat-insulating properties and good mechanical strength to solve the heat-insulating problem of aircraft in actual use. Summary of the invention

[0006] The technical problem solved by the present invention is to provide a honeycomb sandwich structure heat-insulating material and a preparation method thereof, with the aim of solving the defects of existing heat-insulating materials and providing a preparation method of heat-insulating materials so that these components can meet excellent high temperature resistance and heat-insulating properties.

[0007] In order to solve the above problems, the first aspect of the present invention provides a honeycomb sandwich structure heat-insulating material, comprising:

[0008] It comprises a honeycomb core material and a skin layer which are alternately stacked; a glue film is arranged between the honeycomb core material and the skin layer; the honeycomb core material comprises a paper honeycomb core strip and a phthalonitrile resin; the phthalonitrile resin is compounded on the surface and inside of the paper honeycomb core strip;

[0009] The raw materials for preparing the skin layer include reinforcing material and resin solution; the resin solution includes polyimide resin solution and inorganic filler.

[0010] Preferably, the paper honeycomb core strip is a para-aramid paper honeycomb core strip, and the thickness of the paper used to prepare the paper honeycomb core strip is 1 to 10 mm; the heat-resistant temperature of the phthalonitrile resin is higher than 600°C.

[0011] Preferably, the inorganic filler is one of hollow glass microspheres and silica aerogel powder or a mixture of both; the reinforcement fiber cloth is one of quartz glass fiber cloth, glass fiber cloth and hollow quartz glass fiber cloth or a combination of both.

[0012] Preferably, the content of the inorganic filler accounts for 5-50wt% of the content of the polyimide resin; in the skin layer, the total content of the inorganic filler and the polyimide resin is 30-60wt%.

[0013] Preferably, the adhesive film is one or a combination of a quartz-reinforced polyimide adhesive film and a quartz-reinforced modified cyanate ester adhesive film; the thickness of a single layer of the adhesive film is 0.15 to 0.3 mm.

[0014] Preferably, the honeycomb sandwich structure heat-insulating material has a temperature resistance of more than 600°C and a density of 0.2 to 0.8 g / cm 3 , thermal conductivity is not greater than 0.35W / mK; under the thermal test conditions of 600℃ / 120s, the back temperature of the honeycomb sandwich structure thermal insulation material with a thickness of more than 8mm is ≤50℃.

[0015] A second aspect of the present invention provides a method for preparing the honeycomb sandwich structure heat-insulating material as described above, comprising the following steps:

[0016] S1: impregnating paper honeycomb core strips in phthalonitrile solution and then curing to obtain honeycomb core material;

[0017] S2: applying a polyimide resin solution containing an inorganic filler on a reinforcing material to obtain a prepreg, and curing the prepreg to obtain a polyimide skin;

[0018] S3: stacking the polyimide skin, the honeycomb core material and the polyimide skin in sequence along the thickness direction, laying an adhesive film between each layer of the polyimide skin and the honeycomb core material, and then curing to obtain a honeycomb sandwich structure heat-insulating material.

[0019] Preferably, in step S1, the curing temperature is 250-300° C. and the holding time is 1-2 hours.

[0020] Preferably, the thickness of the polyimide skin is 0.1-2 mm.

[0021] Preferably, the curing conditions in step S2 are: heating to 160-200°C, keeping warm for 1-2.5 hours, and a pressure of 0.5-1 MPa; then heating to 240-280°C, keeping warm for 1.5-3 hours, and a pressure of 0.5-1.5 MPa; then heating to 350-450°C, keeping warm for 2-4 hours, and a pressure of 1-2 MPa;

[0022] The curing conditions in step S3 are: curing temperature of 180-300° C., holding time of 1-3 hours, and pressure of 0.5-1.5 MPa.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The honeycomb sandwich structure heat-insulating material of the present invention is prepared by adding inorganic filler hollow glass microspheres or silica aerogel powder into a polyimide matrix. Since the hollow glass microspheres and silica aerogel powder have a relatively low density of 0.1 to 0.5 g / cm 3 And thermal conductivity 0.01~0.04W . m -1 . K -1 Its introduction into polyimide composites can make the material have good thermal insulation and heat preservation functions, while also having the effects of light weight and good mechanical properties.

[0025] The honeycomb sandwich structure heat-insulating material of the present invention introduces a high-temperature resistant honeycomb structure into the structure. The honeycomb structure is a highly efficient lightweight, high-strength, high-rigidity material that can be used as a structural member and can also be used to manufacture functional parts such as heat insulation and noise reduction.

[0026] The honeycomb sandwich structure heat-insulating material of the present invention introduces low-density inorganic fillers and honeycomb structures, and through coupling the two, the advantageous characteristics of the two materials are brought into full play, thereby achieving efficient preparation of lightweight, high-strength, and high-rigidity heat-insulating materials. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] A first aspect of an embodiment of the present invention provides a honeycomb sandwich structure heat-insulating material, comprising:

[0029] It comprises a honeycomb core material and a skin layer which are alternately stacked; a glue film is arranged between the honeycomb core material and the skin layer; the honeycomb core material comprises a paper honeycomb core strip and a phthalonitrile resin; the phthalonitrile resin is compounded on the surface and inside of the paper honeycomb core strip;

[0030] The raw materials for preparing the skin layer include reinforcing material and resin solution; the resin solution includes polyimide resin solution and inorganic filler.

[0031] The honeycomb sandwich structure heat-insulating material of the embodiment of the present invention adds inorganic filler hollow glass microspheres or silica aerogel powder to the polyimide matrix. Since the hollow glass microspheres and silica aerogel powder have a relatively low density of 0.1 to 0.5 g / cm 3 And thermal conductivity 0.01~0.04W . m -1 . K -1 Its introduction into polyimide composites can make the material have good thermal insulation and heat preservation functions, while also having the effects of light weight and good mechanical properties.

[0032] In some embodiments, the paper honeycomb core strip is a para-aramid paper honeycomb core strip, and the thickness of the paper used to prepare the paper honeycomb core strip is 1 to 10 mm; the heat-resistant temperature of the phthalonitrile resin is higher than 600°C.

[0033] In some embodiments, the inorganic filler is a mixture of one or both of hollow glass microspheres and silica aerogel powder; the reinforcement fiber cloth is a combination of one or both of quartz glass fiber cloth, glass fiber cloth and hollow quartz glass fiber cloth.

[0034] In some embodiments, the content of the inorganic filler accounts for 5-50wt% of the content of the polyimide resin; in the skin layer, the total content of the inorganic filler and the polyimide resin is 30-60wt%.

[0035] In some embodiments, the adhesive film is one or a combination of a quartz-reinforced polyimide adhesive film and a quartz-reinforced modified cyanate ester adhesive film; the thickness of a single layer of the adhesive film is 0.15 to 0.3 mm.

[0036] In some embodiments, the honeycomb sandwich structure heat-insulating material has a temperature resistance of above 600°C, a density of 0.2-0.8g / cm3, and a thermal conductivity of no more than 0.35W / mK; under the thermal test conditions of 600°C / 120s, the back temperature of the honeycomb sandwich structure heat-insulating material with a thickness of more than 8mm is ≤50°C.

[0037] A second aspect of an embodiment of the present invention provides a method for preparing the honeycomb sandwich structure heat-insulating material as described above, comprising the following steps:

[0038] S1: impregnating paper honeycomb core strips in phthalonitrile solution and then curing to obtain honeycomb core material;

[0039] S2: applying a polyimide resin solution containing an inorganic filler on a reinforcing material to obtain a prepreg, and curing the prepreg to obtain a polyimide skin;

[0040] S3: stacking the polyimide skin, the honeycomb core material and the polyimide skin in sequence along the thickness direction, laying an adhesive film between each layer of the polyimide skin and the honeycomb core material, and then curing to obtain a honeycomb sandwich structure heat-insulating material.

[0041] In some embodiments, in step S1, the curing temperature is 250-300° C., and the holding time is 1 to 2 hours.

[0042] In some embodiments, the polyimide skin has a thickness of 0.1 to 2 mm.

[0043] In some embodiments, the curing conditions in step S2 are: heating to 160-200° C., keeping warm for 1-2.5 hours, and a pressure of 0.5-1 MPa; then heating to 240-280° C., keeping warm for 1.5-3 hours, and a pressure of 0.5-1.5 MPa; then heating to 350-450° C., keeping warm for 2-4 hours, and a pressure of 1-2 MPa;

[0044] The curing conditions in step S3 are: curing temperature of 180-300° C., holding time of 1-3 hours, and pressure of 0.5-1.5 MPa.

[0045] Example 1

[0046] The honeycomb sandwich structure heat-insulating material of this embodiment includes:

[0047] Alternatingly stacked honeycomb core material and skin layer; a glue film is provided between the honeycomb core material and the skin layer; the honeycomb core material comprises a paper honeycomb core strip with a thickness of 5 mm and a phthalonitrile solution;

[0048] The raw materials for preparing the skin layer include reinforcing materials and resin solution; the resin solution includes 220g of polyimide resin solution and 110g of hollow glass microspheres.

[0049] The method for preparing the honeycomb sandwich structure heat-insulating material of this embodiment comprises the following steps:

[0050] S1: After dipping a 5 mm thick paper honeycomb core strip into a phthalonitrile solution, the solution was cured at 300°C for 1 h to obtain a high temperature resistant honeycomb structure with a thickness of 5 mm;

[0051] S2: 110 g of hollow glass microspheres are added to 220 g of a polyimide resin solution (solid content 50 wt%), and the mixture is stirred to obtain a mixed solution; 330 g of the obtained mixed glue solution is evenly applied on 220 g of a type B quartz glass fiber cloth to prepare a prepreg cloth with a glue content of 50 wt%; the prepared prepreg cloth is cut into fiber prepreg cloth sheets, which are neatly stacked and placed in a mold, and cured under the conditions of keeping the temperature at 160° C. for 1 h, keeping the temperature at 260° C. for 2 h, and keeping the temperature at 380° C. for 2 h to obtain a polyimide skin with a thickness of 0.75 mm containing an inorganic filler;

[0052] S3: The obtained 0.75 mm thick polyimide skin containing inorganic filler is cut into two polyimide skins of the same size; then the aforementioned 0.75 mm thick polyimide skin containing inorganic filler, 5 mm thick high temperature resistant honeycomb core structure and 0.75 mm thick polyimide skin are stacked in sequence along the thickness direction, and a film is laid between each layer of skin and the core material to tightly bond them to form a sandwich structure, which is cured at 200°C for 2 hours to obtain a honeycomb sandwich structure heat-insulating material.

[0053] Example 2

[0054] The honeycomb sandwich structure heat-insulating material of this embodiment includes:

[0055] Alternatingly stacked honeycomb core material and skin layer; a glue film is provided between the honeycomb core material and the skin layer; the honeycomb core material comprises a 6mm thick paper honeycomb core strip and a phthalonitrile solution;

[0056] The raw materials for preparing the skin layer include reinforcing materials and resin solution; the resin solution includes 220g of polyimide resin solution and 110g of hollow glass microspheres.

[0057] The method for preparing the honeycomb sandwich structure heat-insulating material of this embodiment comprises the following steps:

[0058] S1: After dipping a 6 mm thick paper honeycomb core strip into a phthalonitrile solution, the solution was cured at 300°C for 1 h to obtain a 6 mm thick high temperature resistant honeycomb structure;

[0059] S2: 110 g of hollow glass microspheres are added to 220 g of a polyimide resin solution (solid content 50 wt%), and the mixture is stirred to obtain a mixed solution; 330 g of the obtained mixed glue solution is evenly applied on 220 g of a type B quartz glass fiber cloth to prepare a prepreg cloth with a glue content of 50 wt%; the prepared prepreg cloth is cut into fiber prepreg cloth sheets, which are neatly stacked and placed in a mold, and cured under the conditions of keeping the temperature at 160° C. for 1 h, keeping the temperature at 260° C. for 2 h, and keeping the temperature at 380° C. for 2 h to obtain a polyimide skin with a thickness of 0.75 mm containing an inorganic filler;

[0060] S3: The obtained 0.75 mm thick polyimide skin containing inorganic filler is cut into two polyimide skins of the same size; then the aforementioned 0.75 mm thick polyimide skin containing inorganic filler, 6 mm thick high temperature resistant honeycomb core structure and 0.75 mm thick polyimide skin are stacked in sequence along the thickness direction, and a film is laid between each layer of skin and the core material, tightly bonded to form a sandwich structure, and cured at 200°C for 2h to obtain a honeycomb sandwich structure heat-insulating material.

[0061] Example 3

[0062] The honeycomb sandwich structure heat-insulating material of this embodiment includes:

[0063] Alternatingly stacked honeycomb core material and skin layer; a glue film is provided between the honeycomb core material and the skin layer; the honeycomb core material comprises a paper honeycomb core strip with a thickness of 5 mm and a phthalonitrile solution;

[0064] The raw materials for preparing the skin layer include reinforcing materials and resin solution; the resin solution includes 330g of polyimide resin solution and 165g of hollow glass microspheres.

[0065] The method for preparing the honeycomb sandwich structure heat-insulating material of this embodiment comprises the following steps:

[0066] S1: After dipping a 5 mm thick paper honeycomb core strip into a phthalonitrile solution, the solution was cured at 300°C for 1 h to obtain a high temperature resistant honeycomb structure with a thickness of 5 mm;

[0067] S2: 165 g of hollow glass microspheres are added to 330 g of polyimide resin solution (solid content 50 wt%), and the mixture is obtained after being stirred evenly; 495 g of the obtained mixed glue solution is evenly applied on 220 g of type B quartz glass fiber cloth to prepare a prepreg cloth with a glue content of 60 wt%; the prepared prepreg cloth is cut into fiber prepreg cloth sheets, which are neatly stacked and placed in a mold, and cured under the conditions of keeping the temperature at 160° C. for 1 h, keeping the temperature at 260° C. for 2 h, and keeping the temperature at 380° C. for 2 h to obtain a polyimide skin with a thickness of 0.75 mm containing inorganic fillers;

[0068] S3: The obtained 0.75 mm thick polyimide skin containing inorganic filler is cut into two polyimide skins of the same size; then the aforementioned 0.75 mm thick polyimide skin containing inorganic filler, 5 mm thick high temperature resistant honeycomb core structure and 0.75 mm thick polyimide skin are stacked in sequence along the thickness direction, and adhesive film is laid between each layer of skin and the core material, tightly bonded to form a sandwich structure, and cured at 200°C for 2h to obtain a honeycomb sandwich structure heat-insulating material.

[0069] Example 4

[0070] The honeycomb sandwich structure heat-insulating material of this embodiment includes:

[0071] Alternatingly stacked honeycomb core material and skin layer; a glue film is provided between the honeycomb core material and the skin layer; the honeycomb core material comprises a paper honeycomb core strip with a thickness of 5 mm and a phthalonitrile solution;

[0072] The raw materials for preparing the skin layer include reinforcing materials and resin solution; the resin solution includes 220g of polyimide resin solution and 110g of hollow glass microspheres.

[0073] The method for preparing the honeycomb sandwich structure heat-insulating material of this embodiment comprises the following steps:

[0074] S1: After dipping a 5 mm thick paper honeycomb core strip into a phthalonitrile solution, the solution was cured at 300°C for 1 h to obtain a high temperature resistant honeycomb structure with a thickness of 5 mm;

[0075] S2: 110 g of hollow glass microspheres are added to 220 g of a polyimide resin solution (solid content 50 wt%), and the mixture is obtained after being stirred evenly; 330 g of the obtained mixed glue solution is evenly applied on 220 g of a type B quartz glass fiber cloth to prepare a prepreg cloth with a glue content of 50 wt%; the prepared prepreg cloth is cut into fiber prepreg cloth sheets, which are neatly stacked and placed in a mold, and cured under the conditions of being kept at 160° C. for 1 h, at 260° C. for 2 h, and at 380° C. for 2 h to obtain a polyimide skin with a thickness of 1.5 mm containing an inorganic filler;

[0076] S3: The obtained 1.5 mm thick polyimide skin containing inorganic filler is cut into 2 polyimide skins of the same size; then the aforementioned 1.5 mm thick polyimide skin containing inorganic filler, 5 mm thick high temperature resistant honeycomb core structure and 1.5 mm thick polyimide skin are stacked in sequence along the thickness direction, and a film is laid between each layer of skin and the core material, tightly bonded to form a sandwich structure, and cured at 200°C for 2h to obtain a honeycomb sandwich structure heat-insulating material.

[0077] Example 5

[0078] The honeycomb sandwich structure heat-insulating material of this embodiment includes:

[0079] Alternatingly stacked honeycomb core material and skin layer; a glue film is provided between the honeycomb core material and the skin layer; the honeycomb core material comprises a 6mm thick paper honeycomb core strip and a phthalonitrile solution;

[0080] The raw materials for preparing the skin layer include reinforcing materials and resin solution; the resin solution includes 330g of polyimide resin solution and 165g of hollow glass microspheres.

[0081] The method for preparing the honeycomb sandwich structure heat-insulating material of this embodiment comprises the following steps:

[0082] S1: After dipping a 6 mm thick paper honeycomb core strip into a phthalonitrile solution, the solution was cured at 300°C for 1 h to obtain a 6 mm thick high temperature resistant honeycomb structure;

[0083] S2: 165 g of hollow glass microspheres were added to 330 g of polyimide resin solution (solid content 50 wt%), and the mixture was obtained after being stirred evenly; 495 g of the obtained mixed glue solution was evenly applied on 220 g of type B quartz glass fiber cloth to prepare a prepreg cloth with a glue content of 60 wt%; the prepared prepreg cloth was cut into fiber prepreg cloth sheets, which were neatly stacked and placed in a mold, and cured under the conditions of keeping the temperature at 160° C. for 1 h, keeping the temperature at 260° C. for 2 h, and keeping the temperature at 380° C. for 2 h to obtain a polyimide skin with a thickness of 1.5 mm containing inorganic fillers;

[0084] S3: The obtained 1.5 mm thick polyimide skin containing inorganic filler is cut into 2 polyimide skins of the same size; then the aforementioned 1.5 mm thick polyimide skin containing inorganic filler, 6 mm thick high temperature resistant honeycomb core structure and 1.5 mm thick polyimide skin are stacked in sequence along the thickness direction, and adhesive film is laid between each layer of skin and the core material, tightly bonded to form a sandwich structure, and cured at 200°C for 2h to obtain a honeycomb sandwich structure heat insulation material.

[0085] Example 6

[0086] The honeycomb sandwich structure heat-insulating material of this embodiment includes:

[0087] Alternatingly stacked honeycomb core material and skin layer; a glue film is provided between the honeycomb core material and the skin layer; the honeycomb core material comprises a 6mm thick paper honeycomb core strip and a phthalonitrile solution;

[0088] The raw materials for preparing the skin layer include reinforcing materials and resin solution; the resin solution includes 600g of polyimide resin solution and 30g of hollow glass microspheres.

[0089] The method for preparing the honeycomb sandwich structure heat-insulating material of this embodiment comprises the following steps:

[0090] S1: After dipping a 6 mm thick paper honeycomb core strip into a phthalonitrile solution, the solution was cured at 300°C for 1 h to obtain a 6 mm thick high temperature resistant honeycomb structure;

[0091] S2: 30 g of hollow glass microspheres are added to 600 g of polyimide resin solution (solid content 50 wt%), and the mixture is stirred to obtain a mixed solution; the obtained 630 g of mixed glue solution is evenly applied on 220 g of type B quartz glass fiber cloth to prepare a prepreg cloth with a glue content of 60 wt%; the prepared prepreg cloth is cut into fiber prepreg cloth sheets, which are neatly stacked and placed in a mold, and cured under the conditions of keeping the temperature at 160° C. for 1 h, keeping the temperature at 260° C. for 2 h, and keeping the temperature at 380° C. for 2 h to obtain a polyimide skin with a thickness of 1.5 mm containing inorganic fillers;

[0092] S3: The obtained 1.5 mm thick polyimide skin containing inorganic filler is cut into 2 polyimide skins of the same size; then the aforementioned 1.5 mm thick polyimide skin containing inorganic filler, 6 mm thick high temperature resistant honeycomb core structure and 1.5 mm thick polyimide skin are stacked in sequence along the thickness direction, and adhesive film is laid between each layer of skin and the core material, tightly bonded to form a sandwich structure, and cured at 200°C for 2h to obtain a honeycomb sandwich structure heat insulation material.

[0093] Example 7

[0094] The honeycomb sandwich structure heat-insulating material of this embodiment includes:

[0095] Alternatingly stacked honeycomb core material and skin layer; a glue film is provided between the honeycomb core material and the skin layer; the honeycomb core material comprises a 6mm thick paper honeycomb core strip and a phthalonitrile solution;

[0096] The raw materials for preparing the skin layer include reinforcing materials and resin solution; the resin solution includes 300g of polyimide resin solution and 180g of hollow glass microspheres.

[0097] The method for preparing the honeycomb sandwich structure heat-insulating material of this embodiment comprises the following steps:

[0098] S1: After dipping a 6 mm thick paper honeycomb core strip into a phthalonitrile solution, the solution was cured at 300°C for 1 h to obtain a 6 mm thick high temperature resistant honeycomb structure;

[0099] S2: 180 g of hollow glass microspheres are added to 300 g of polyimide resin solution (solid content 50 wt%), and the mixture is stirred to obtain a mixed solution; 480 g of the obtained mixed glue solution is evenly applied on 220 g of type B quartz glass fiber cloth to prepare a prepreg cloth with a glue content of 60 wt%; the prepared prepreg cloth is cut into fiber prepreg cloth sheets, which are neatly stacked and placed in a mold, and cured under the conditions of keeping the temperature at 160° C. for 1 h, keeping the temperature at 260° C. for 2 h, and keeping the temperature at 380° C. for 2 h to obtain a polyimide skin with a thickness of 1.5 mm containing inorganic fillers;

[0100] S3: The obtained 1.5 mm thick polyimide skin containing inorganic filler is cut into 2 polyimide skins of the same size; then the aforementioned 1.5 mm thick polyimide skin containing inorganic filler, 6 mm thick high temperature resistant honeycomb core structure and 1.5 mm thick polyimide skin are stacked in sequence along the thickness direction, and adhesive film is laid between each layer of skin and the core material, tightly bonded to form a sandwich structure, and cured at 200°C for 2h to obtain a honeycomb sandwich structure heat insulation material.

[0101] Example 8

[0102] The honeycomb sandwich structure heat-insulating material of this embodiment includes:

[0103] Alternatingly stacked honeycomb core material and skin layer; a glue film is provided between the honeycomb core material and the skin layer; the honeycomb core material comprises a 6mm thick paper honeycomb core strip and a phthalonitrile solution;

[0104] The raw materials for preparing the skin layer include reinforcing material and resin solution; the resin solution includes 330g of polyimide resin solution and 165g of silica aerogel powder.

[0105] The method for preparing the honeycomb sandwich structure heat-insulating material of this embodiment comprises the following steps:

[0106] S1: After dipping a 6 mm thick paper honeycomb core strip into a phthalonitrile solution, the solution was cured at 300°C for 1 h to obtain a 6 mm thick high temperature resistant honeycomb structure;

[0107] S2: 165 g of silica aerogel powder was added to 330 g of polyimide resin solution (solid content 50 wt%), and the mixture was obtained after being stirred evenly; 495 g of the obtained mixed glue solution was evenly applied on 220 g of type B quartz glass fiber cloth to prepare a prepreg cloth with a glue content of 60 wt%; the prepared prepreg cloth was cut into fiber prepreg cloth sheets, which were neatly stacked and placed in a mold, and cured under the conditions of keeping the temperature at 160° C. for 1 h, keeping the temperature at 260° C. for 2 h, and keeping the temperature at 380° C. for 2 h to obtain a polyimide skin with a thickness of 1.5 mm containing inorganic fillers;

[0108] S3: The obtained 1.5 mm thick polyimide skin containing inorganic filler is cut into 2 polyimide skins of the same size; then the aforementioned 1.5 mm thick polyimide skin containing inorganic filler, 6 mm thick high temperature resistant honeycomb core structure and 1.5 mm thick polyimide skin are stacked in sequence along the thickness direction, and adhesive film is laid between each layer of skin and the core material, tightly bonded to form a sandwich structure, and cured at 200°C for 2h to obtain a honeycomb sandwich structure heat insulation material.

[0109] Comparative Example 1

[0110] The difference between this comparative example and Example 1 is that no inorganic filler is added.

[0111] Comparative Example 2

[0112] The difference between this comparative example and Example 1 is that the inorganic filler is silicon carbide powder.

[0113] Table 1 Mechanical properties test of honeycomb sandwich structure thermal insulation materials

[0114]

[0115] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A honeycomb sandwich structure heat-insulating material, characterized by: It comprises a honeycomb core material and a skin layer which are alternately stacked; a glue film is arranged between the honeycomb core material and the skin layer; the honeycomb core material comprises a paper honeycomb core strip and a phthalonitrile resin; the phthalonitrile resin is compounded on the surface and inside of the paper honeycomb core strip; The raw materials for preparing the skin layer include reinforcing material and resin solution; the resin solution includes polyimide resin solution and inorganic filler.

2. The honeycomb sandwich structure heat-insulating material according to claim 1, characterized in that: The paper honeycomb core strip is a para-aramid paper honeycomb core strip, and the thickness of the paper used to prepare the paper honeycomb core strip is 1-10 mm; the heat-resistant temperature of the phthalonitrile resin is higher than 600°C.

3. The honeycomb sandwich structure heat-insulating material according to claim 1, characterized in that: The inorganic filler is one or a mixture of hollow glass microspheres and silica aerogel powder; The reinforcement fiber cloth is one of quartz glass fiber cloth, glass fiber cloth and hollow quartz glass fiber cloth, or a combination of two of them.

4. The honeycomb sandwich structure heat-insulating material according to claim 1, characterized in that: The content of the inorganic filler accounts for 5-50wt% of the polyimide resin content; in the skin layer, the total content of the inorganic filler and the polyimide resin is 30-60wt%.

5. The honeycomb sandwich structure heat-insulating material according to claim 1, characterized in that: The adhesive film is one or a combination of quartz-reinforced polyimide adhesive film and quartz-reinforced modified cyanate ester adhesive film; the thickness of a single layer of the adhesive film is 0.15-0.3 mm.

6. The honeycomb sandwich structure heat-insulating material according to claim 1, characterized in that: The honeycomb sandwich structure heat-insulating material has a temperature resistance of more than 600°C and a density of 0.2 to 0.8 g / cm 3 , thermal conductivity is not greater than 0.35W / mK; under the thermal test conditions of 600℃ / 120s, the back temperature of the honeycomb sandwich structure thermal insulation material with a thickness of more than 8mm is ≤50℃.

7. A method for preparing a honeycomb sandwich structure heat-insulating material according to any one of claims 1 to 6, characterized in that: The steps include: S1: impregnating paper honeycomb core strips in phthalonitrile solution and then curing to obtain honeycomb core material; S2: applying a polyimide resin solution containing an inorganic filler on a reinforcing material to obtain a prepreg, and curing the prepreg to obtain a polyimide skin; S3: stacking the polyimide skin, the honeycomb core material and the polyimide skin in sequence along the thickness direction, laying an adhesive film between each layer of the polyimide skin and the honeycomb core material, and then curing to obtain a honeycomb sandwich structure heat-insulating material.

8. The method for preparing the honeycomb sandwich structure heat-insulating material according to claim 7, characterized in that: In the step S1, the curing temperature is 250-300° C. and the heat preservation time is 1-2 hours.

9. The method for preparing the honeycomb sandwich structure heat-insulating material according to claim 7, characterized in that: The thickness of the polyimide skin is 0.1-2 mm.

10. The method for preparing the honeycomb sandwich structure heat-insulating material according to claim 7, characterized in that: The curing conditions in step S2 are: heating to 160-200°C, keeping warm for 1-2.5 hours, and a pressure of 0.5-1 MPa; then heating to 240-280°C, keeping warm for 1.5-3 hours, and a pressure of 0.5-1.5 MPa; then heating to 350-450°C, keeping warm for 2-4 hours, and a pressure of 1-2 MPa; The curing conditions in step S3 are: curing temperature of 180-300° C., holding time of 1-3 hours, and pressure of 0.5-1.5 MPa.

Citation Information

Patent Citations

  • Aramid paper honeycomb sandwich composite structure with high strength and light weight

    CN105882016A

  • Interlayer structure composite material and preparation method thereof

    CN106113738A

  • Preparation method of large-size high-temperature-resistant honeycomb

    CN113635612A

  • High-temperature composite honeycomb

    CN114126852A

  • Silicon dioxide aerogel, quartz fiber and polyimide ternary composite material as well as preparation method and application thereof

    CN115449219A