Spherical lithium hydroxide and preparation method and application thereof

The preparation of spherical lithium hydroxide through coating powder solution and rolling ball technology solves the problems of high cost of lithium hydroxide dust and high cost in confined spaces, achieving efficient carbon dioxide absorption and low dust effects, which is suitable for the carbon dioxide removal needs in confined spaces.

CN119059537APending Publication Date: 2024-12-03THE 718TH RES INST OF CHINA STATE SHIPBUILDING CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410955590.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the existing carbon dioxide removal method in confined space, the absorption efficiency of alkali lime is low and easy to be deactivated. Lithium hydroxide dust has a high stimulation to the human body and is costly. It is necessary to develop low-cost, low-dust high-efficiency carbon dioxide absorbers.

Method used

Single water lithium hydroxide is used as raw material, and spherical lithium hydroxide is prepared through coating powder solution and rolling ball technology. Through batch spray granulation and drying processes, a spherical lithium hydroxide absorber with high strength and low dust is formed.

Benefits of technology

It achieves efficient carbon dioxide absorption performance, reduces the risk of lithium hydroxide dust, and is cheap in process, suitable for mass production, improving the comfort of personnel in confined spaces.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of closed space atmospheric environment control, and particularly relates to spherical lithium hydroxide and a preparation method and application thereof, and the preparation method comprises the following steps: 1) dissolving coating powder in water to obtain a coating powder solution; 2) adding the lithium hydroxide monohydrate powder into a granulator, starting equipment, adding the coating powder solution in an intermittent spraying manner, and granulating; 3) continuing to add a proper amount of lithium hydroxide monohydrate powder into the granulator, then adding a coating powder solution in an intermittent spraying manner, and coating the surface of the sphere with the lithium hydroxide monohydrate powder; (4) repeating the step (3) until the designed dosage of the lithium hydroxide monohydrate powder is reached; (5) screening spherical lithium hydroxide with the particle size of 2-4mm; and 6) drying the spherical lithium hydroxide with the particle size of 2-4 mm. The preparation method is simple, feasible and low in cost, and the prepared spherical lithium hydroxide has the advantages of high strength, low dust rate and high carbon dioxide absorption efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of air environment control in confined spaces, and in particular relates to spherical lithium hydroxide and a preparation method and application thereof. Background Art

[0002] The control of the atmospheric environment in confined spaces such as space stations, spacecraft, submarines, personal submersibles, mobile lifeboats in coal mines, and emergency refuge chambers is a basic condition for ensuring the safety of personnel, and the removal of carbon dioxide is of utmost importance. At present, the methods for removing carbon dioxide in confined spaces mainly include chemical systems using alkaline agents such as lithium hydroxide, soda lime, Bahrain lime, and organic amines, and physical adsorption systems such as molecular sieves, alumina, and gels. Considering practicality and feasibility, only chemical absorption systems are currently suitable for removing carbon dioxide in confined spaces.

[0003] The theoretical absorption rate of soda lime for carbon dioxide is 78.6%, but the absorption efficiency is low and it is very easy to be deactivated and lose its absorption capacity. Therefore, it is necessary to equip enough soda lime absorbents to ensure emergency needs. This will greatly reduce the flexibility of combat equipment; and the moisture produced during the absorption process causes the environmental humidity to increase rapidly, resulting in low comfort for trainees. Relatively speaking, lithium hydroxide has the highest carbon dioxide absorption rate, with a theoretical value of up to 91.7%. Its carbon dioxide absorption capacity is 2.5 times that of the same mass of soda lime, which can greatly reduce the amount of charge. At the same time, lithium hydroxide can absorb moisture in the environment to form lithium hydroxide monohydrate, which effectively reduces the environmental humidity. It can also absorb some toxic gases such as chlorine, which significantly improves the environmental comfort of trainees.

[0004] However, since lithium hydroxide dust is highly irritating to the human respiratory tract, especially in confined spaces, researchers still need to develop absorbents with appropriate structures to reduce the dust rate of lithium hydroxide, effectively prevent dust from the absorbent, and improve the comfort of people in confined spaces. In addition, due to the high cost of lithium hydroxide raw materials, low-cost processes for preparing lithium hydroxide absorbents need to be given priority. Summary of the invention

[0005] The object of the present invention is to provide a spherical lithium hydroxide and a preparation method and application thereof. The preparation method uses lithium hydroxide monohydrate as a raw material and a coating powder solution as a medium. The fine powder of lithium hydroxide monohydrate is bonded layer by layer to form spherical lithium hydroxide by rolling a ball. The preparation method is simple and feasible with low cost. The prepared spherical lithium hydroxide has the advantages of high strength, low dust rate and high carbon dioxide absorption efficiency.

[0006] Specifically, the present invention provides the following technical solutions:

[0007] A method for preparing spherical lithium hydroxide comprises the following steps:

[0008] 1) dissolving the coating powder in water to obtain a coating powder solution;

[0009] 2) adding lithium hydroxide monohydrate powder to a granulator, starting the equipment, and then adding water by intermittent spraying to perform granulation; the intermittent spraying method of adding water is as follows: during the granulation process, the material is uniformly sprayed every 1-5 minutes for 5-40 seconds;

[0010] 3) continuing to add an appropriate amount of lithium hydroxide monohydrate powder to the granulator, and then adding water by intermittent spraying to coat the lithium hydroxide monohydrate powder on the surface of the sphere; the intermittent spraying method of adding water is specifically: uniformly spraying the material every 1-5 minutes for 5-40 seconds;

[0011] 4) Repeat step 3) until the designed amount of lithium hydroxide monohydrate powder is reached;

[0012] 5) Screening out spherical lithium hydroxide with a particle size of 2-4 mm;

[0013] 6) Drying the spherical lithium hydroxide with a particle size of 2-4 mm to obtain.

[0014] Preferably, in step 1), the coating powder is selected from at least one of hydroxypropyl cellulose, hydroxypropyl methyl cellulose, acrylic resin IV, polyvinyl pyrrolidone, and polyvinyl acetal diethylamine acetic acid.

[0015] More preferably, the coating powder is a combination of hydroxypropyl cellulose, hydroxypropyl methyl cellulose, acrylic resin IV, polyvinyl pyrrolidone, and polyvinyl acetaldehyde diethylamine acetic acid; studies have found that combining the above-mentioned coating powders together has a better spheronization effect.

[0016] Preferably, in step 1), the concentration of the coating powder solution is 1-15 wt %. If the concentration is too high, it will be difficult to atomize.

[0017] Preferably, in step 2) and step 3), the particle size of the lithium hydroxide monohydrate is 5-80 microns, more preferably 5-30 microns. Studies have found that using lithium hydroxide monohydrate in the above particle size range as a raw material, the surface of the prepared spherical lithium hydroxide is more rounded, which is conducive to enhancing the strength of the spherical lithium hydroxide.

[0018] Preferably, in step 2), the granulator is a round pan granulator or a disc granulator.

[0019] Preferably, in step 2), the weight of the lithium hydroxide monohydrate powder initially added is 25-50% of the designed amount.

[0020] Preferably, in step 3), the weight of lithium hydroxide monohydrate powder added each time is 5-15% of the designed amount.

[0021] The present invention achieves effective control over the particle size of the prepared spherical lithium hydroxide by limiting the initial addition amount and the subsequent single addition amount of lithium hydroxide monohydrate powder, as well as the method of adding water, and can ensure that the proportion of 2-4 mm spherical lithium hydroxide produced in a single production reaches between 75-95%.

[0022] Preferably, in step 2), the amount of water added is 5-15% of the mass of the lithium hydroxide monohydrate powder added in step 1).

[0023] Preferably, in step 3), the amount of water added is 5-15% of the mass of the lithium hydroxide monohydrate powder added in step 2).

[0024] Preferably, in step 5), the spherical lithium hydroxide with a particle size greater than 4 mm is ground and mixed with the spherical lithium hydroxide with a particle size less than 2 mm, and ground, and the process returns to step 2) for granulation.

[0025] Preferably, in step 6), the drying temperature is 100-180° C. and the drying time is 2-15 hours.

[0026] More preferably, the drying temperature is 130-160° C. and the drying time is 9-12 hours.

[0027] The present invention also provides spherical lithium hydroxide, which is prepared by the above-mentioned preparation method.

[0028] The present invention also provides the use of the spherical lithium hydroxide in adsorbing carbon dioxide.

[0029] The beneficial effects of the present invention are at least:

[0030] 1) The present invention provides a method for preparing spherical lithium hydroxide, which has a simple and efficient preparation process, low cost, and no waste is generated during the preparation process, thereby achieving efficient utilization of high-value lithium hydroxide materials and reducing the impact of strongly alkaline lithium hydroxide powder on the environment;

[0031] 2) The present invention provides a method for preparing spherical lithium hydroxide, which uses a coating powder solution as a medium, so that the ball-forming speed of lithium hydroxide monohydrate powder is significantly accelerated, the process stability is high, and the ball-forming efficiency is high;

[0032] 3) The present invention provides a method for preparing spherical lithium hydroxide, which forms spherical lithium hydroxide by bonding lithium hydroxide monohydrate fine powder layer by layer through rolling balls and adding coating powder solution to form spherical lithium hydroxide, thereby ensuring that the spherical lithium hydroxide has high strength and is not prone to slag and lithium hydroxide dust that may cause harm to users;

[0033] 4) The present invention provides a method for preparing spherical lithium hydroxide, wherein the water content of lithium hydroxide monohydrate powder exceeds 43%. When the wet ball is dried, a large number of gas channels will be left in the spherical lithium hydroxide after the water evaporates, which will greatly increase the contact area between the spherical lithium hydroxide and the carbon dioxide reaction, and greatly improve the carbon dioxide absorption performance of the spherical lithium hydroxide;

[0034] 5) The present invention provides a method for preparing spherical lithium hydroxide. The prepared spherical lithium hydroxide product has a high bulk density after filling, occupies a small volume, and the gaps between different small balls are evenly distributed, and there will be no problem of local gas blockage and short circuit that reduces the carbon dioxide absorption performance. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention is described clearly and completely below. The following embodiments are used to illustrate the present invention, but are not used to limit the scope of the present invention. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in the field or the product instructions are used.

[0036] In the following examples, the industrial-grade lithium hydroxide monohydrate powder used was sourced from Sichuan Yahua Lithium Technology Co., Ltd.

[0037] In the following embodiments, the round pot granulator used is from: Zhengzhou Rongkai Machinery Equipment Co., Ltd., model 100, and in working state, the speed is controlled to be 10-40r / min, and the inclination angle is controlled within the range of 20-35 degrees.

[0038] Example 1

[0039] (1) Dissolving the coating powder in water to obtain a coating powder solution with a concentration of 1 wt %; wherein the coating powder components are hydroxypropyl cellulose, hydroxypropyl methyl cellulose, acrylic resin IV, polyvinyl pyrrolidone, and polyvinyl acetal diethylamine acetic acid, which are prepared in a mass ratio of 10:10:3:1:1 and configured in a certain proportion, the same below.

[0040] (2) 10 kg of industrial-grade lithium hydroxide monohydrate powder with a particle size of 5-30 μm was added to a round pot granulator, the equipment was started, and the coating powder solution was sprayed onto the material in the equipment by intermittent spraying. The material was evenly sprayed every 3 minutes for 20 seconds, and the final amount of liquid added was controlled to be 1.4 kg, so that all the powder was wetted and balled into a sphere;

[0041] (3) Add 1 kg of lithium hydroxide monohydrate powder to the round pot granulator again, and spray the coating powder solution onto the material in the equipment by intermittent spraying. Spray the material evenly every 3 minutes for 10 seconds, and finally control the amount of liquid added to 140 g;

[0042] (4) Repeat step 3) until the total amount of lithium hydroxide monohydrate powder added reaches 20 kg (Note: after the last addition of 1 kg of lithium hydroxide monohydrate powder, 140 g of coating powder solution still needs to be sprayed in by intermittent spraying);

[0043] (5) Using a vibrating screen machine with a sieve size of 2 mm and 4 mm, sieving out spherical lithium hydroxide with a particle size of 2-4 mm, and grinding the spherical lithium hydroxide with a particle size greater than 4 mm, mixing it with the spherical lithium hydroxide powder with a particle size less than 2 mm and retaining it, which can be directly used for the next pot of lithium hydroxide pelletizing;

[0044] (6) The screened spherical lithium hydroxide with a size of 2-4 mm is transferred to a forced air oven and dried at 100° C. for 15 hours. After drying, the water content of the spherical lithium hydroxide is detected to be less than 0.5%. The prepared spherical lithium hydroxide is then vacuum packaged.

[0045] Example 2

[0046] (1) dissolving the coating powder in water to obtain a coating powder solution with a concentration of 15 wt %;

[0047] (2) 15 kg of industrial-grade lithium hydroxide monohydrate powder with a particle size of 5-80 μm was added to a round pot granulator, the equipment was started, and the coating powder solution was sprayed onto the material in the equipment by intermittent spraying. The material was evenly sprayed every 5 minutes for 40 seconds, and the final amount of liquid added was controlled to be 2 kg, so that all the powder was wetted and balled into a sphere;

[0048] (3) Add 2 kg of lithium hydroxide monohydrate powder to the round pot granulator again, and spray the coating powder solution onto the material in the equipment by intermittent spraying. Spray the material evenly for 30 seconds every 5 minutes, and finally control the amount of liquid added to 200 g;

[0049] (4) Repeat step 3) until the total amount of lithium hydroxide monohydrate powder added reaches 30 kg (Note: after the last addition of 1 kg of lithium hydroxide monohydrate powder, 100 g of coating powder solution still needs to be sprayed in by intermittent spraying);

[0050] (5) Using a vibrating screen machine with a sieve size of 2 mm and 4 mm, sieving out spherical lithium hydroxide with a particle size of 2-4 mm, and grinding the spherical lithium hydroxide with a particle size greater than 4 mm, mixing it with the spherical lithium hydroxide powder with a particle size less than 2 mm and retaining it, which can be directly used for the next pot of lithium hydroxide pelletizing;

[0051] (6) The screened spherical lithium hydroxide with a size of 2-4 mm is transferred to a forced air oven and dried at 150° C. for 8 hours. After drying, the water content of the spherical lithium hydroxide is detected to be less than 0.5%. The prepared spherical lithium hydroxide is then vacuum packaged.

[0052] Example 3

[0053] (1) dissolving the coating powder in water to obtain a coating powder solution with a concentration of 5%;

[0054] (2) Take 5 kg of industrial-grade lithium hydroxide monohydrate powder with a particle size of 5-80 μm, add it to a round pot granulator, start the equipment, and spray the coating powder solution onto the material in the equipment by intermittent spraying. Spray the material evenly every 2 minutes for 5 seconds, and finally control the amount of liquid added to 250 g, so that all the powder is wetted and balled into a ball;

[0055] (3) Add 1 kg of lithium hydroxide monohydrate powder to the round pot granulator again, and spray the coating powder solution onto the material in the equipment by intermittent spraying. Spray the material evenly every 2 minutes for 10 seconds, and finally control the amount of liquid added to 50 g;

[0056] (4) Repeat step 3) until the total amount of lithium hydroxide monohydrate powder added reaches 20 kg (Note: after the last addition of 1 kg of lithium hydroxide monohydrate powder, 50 g of coating powder solution must be sprayed in intermittently, and the equipment can be stopped after continuing to operate for 5 minutes);

[0057] (5) Using a vibrating screen machine with a sieve size of 2 mm and 4 mm, sieving out spherical lithium hydroxide with a particle size of 2-4 mm, and grinding the spherical lithium hydroxide with a particle size greater than 4 mm, mixing it with the spherical lithium hydroxide powder with a particle size less than 2 mm and retaining it, which can be directly used for the next pot of lithium hydroxide pelletizing;

[0058] (6) The screened spherical lithium hydroxide with a size of 2-4 mm is transferred to a forced air oven and dried at 180° C. for 2 hours. After drying, the water content of the spherical lithium hydroxide is detected to be less than 0.5%. The prepared spherical lithium hydroxide is then vacuum packaged.

[0059] The spherical lithium hydroxide prepared by the method of the present invention has excellent carbon dioxide absorption performance, high absorption efficiency, long effective absorption time, round and regular particle size, high stacking density and high particle strength, is not easy to generate dust during transportation and use, and is beneficial to improving the comfort of users; at the same time, the manufacturing cost of the spherical lithium hydroxide is low and can be mass-produced.

[0060] Comparative Example 1

[0061] Compared with Example 1, the only difference is that the concentration of the coating powder prepared in step 1) is 20wt%.

[0062] Comparative Example 1: The pelletization was carried out according to the steps in Example 1. It was found that when the concentration of the coating powder was too high, the high-pressure atomization effect was poor, and the sprayed binding liquid was in the form of lines rather than mist. Therefore, the powder in the equipment would be adhered to form large lumps and could not be efficiently pelletized.

[0063] Comparative Example 2

[0064] Compared with Example 2, the only difference is that the particle size of the lithium hydroxide monohydrate raw material is 200-500 microns.

[0065] Comparative Example 2: Balling was carried out according to the steps and methods in Example 1. It was found that when the raw material particle size was too large, the powder was difficult to agglomerate into balls, the balling ratio was low, and the surface of the lithium hydroxide after balling was rough and the particle strength was low.

[0066] Comparative Example 3

[0067] Compared with Example 2, the only difference is that the amount of water added in step 2) and step 3) is 20% of the mass of the lithium hydroxide monohydrate powder added in the step.

[0068] The results showed that a large amount of powder in the equipment stuck to the pot, resulting in a low ball formation rate, and the spherical lithium hydroxide was prone to breakage during the operation of the equipment.

[0069] Comparative Example 4

[0070] Compared with Example 2, the only difference is that the amount of water added in step 2) and step 3) is 3% of the mass of the lithium hydroxide monohydrate powder added in the step.

[0071] The results showed that there was a large amount of lithium hydroxide powder in the equipment, which could not participate in the pelletizing process, resulting in a low pelletizing rate.

[0072] Comparative Example 5

[0073] Compared with Example 1, the only difference is that the spherical lithium hydroxide with a particle size of less than 2 mm screened out in step 5) is used as the final product for drying in step 6).

[0074] Experimental tests have shown that the carbon dioxide absorption performance of spherical lithium hydroxide with a particle size of less than 2 mm is poor and cannot meet practical applications. This is mainly because the stacking density of spherical lithium hydroxide with a particle size of less than 2 mm is high, and the tight stacking causes the flow of carbon dioxide gas to be blocked and cannot be quickly absorbed.

[0075] Comparative Example 6

[0076] Compared with Example 1, the only difference is that the spherical lithium hydroxide with a particle size greater than 4 mm screened out in step 5) is used as the final product and is dried in step 6).

[0077] Experimental tests show that the carbon dioxide absorption performance of spherical lithium hydroxide with a particle size of more than 4 mm is also poor and cannot meet practical applications. This is mainly because the specific surface area of ​​spherical lithium hydroxide with a particle size greater than 4 mm is relatively low. Affected by gas diffusion, the lithium hydroxide in the inner core of the sphere is difficult to participate in the carbon dioxide reaction, resulting in a decrease in absorption performance.

[0078] Test example

[0079] First, in order to verify the performance of the prepared spherical lithium hydroxide in practical applications, 40m 3 The closed cabin is used to complete the carbon dioxide absorption performance test of spherical lithium hydroxide. 5.3kg of spherical lithium hydroxide reagent is canned and placed in the corresponding device. When the carbon dioxide concentration in the closed cabin reaches 0.7%, the device is turned on to start the test and record the change of carbon dioxide concentration in the closed cabin with the absorption time. During the test, the ventilation volume of carbon dioxide is controlled to be 0.2m3 / h, and the test is ended when the carbon dioxide concentration reaches 0.7% again. According to the conventional use requirements of the product, it is necessary to ensure that the absorbent controls the carbon dioxide concentration to be lower than 0.7% for an absorption time of more than 10 hours. After multiple closed cabin absorption performance tests, the results show that the effective absorption time of the spherical lithium hydroxide prepared by the present invention exceeds 10 hours, and the absorption time of the samples with better performance exceeds 10.5 hours. Specifically, the specific absorption times of Examples 1-3 are 10 hours and 42 minutes, 10 hours and 15 minutes, and 10 hours and 18 minutes, respectively.

[0080] Secondly, according to the requirements of GJB 8040-2013 carbon dioxide absorbent specification standard, the carbon dioxide absorption rate of spherical lithium hydroxide was determined. After multiple tests, the results showed that the absorption rate of spherical lithium hydroxide was higher than 85%. Specifically, the absorption rates of Examples 1-3 were 86.4%, 85.2%, and 85.7%, respectively, which were significantly better than other lithium hydroxide products reported in the literature; by testing the composition of spherical lithium hydroxide, the results showed that the lithium hydroxide content in the spherical lithium hydroxide ranged from 95 to 97.5wt%.

[0081] Then, the strength of the spherical lithium hydroxide was tested, and the test method was as follows: take a spherical lithium hydroxide sample with a beaker, pass it through a standard sieve with a pore size of 2.0 mm, weigh 20.00 g of the sieved spherical lithium hydroxide sample with an electronic balance, and put it into a strength test rotating device. A spherical object (about 1 cm in diameter) for testing is placed in the device, which is used to collide and rub with the spherical lithium hydroxide in a rotating state to test the strength of the spherical lithium hydroxide particles. Start the strength test rotating device, close it after 15 minutes, pour out the spherical lithium hydroxide sample and pass it through a standard sieve with a pore size of 2.0 mm, weigh the weight of the remaining granules on the sieve to calculate the weight change before and after the test, and the strength value is equal to the weight of the remaining granules on the sieve divided by the weight of the spherical lithium hydroxide added. The test results show that the strength values ​​of the spherical lithium hydroxide prepared in Examples 1-3 are all higher than 99.5%. It shows that the strengthening effect of the coating powder solution further improves the strength of the spherical lithium hydroxide.

[0082] Finally, the dust rate of canned spherical lithium hydroxide during use was determined according to actual use conditions, mainly to test whether the LiOH aerosol concentration in the closed cabin is less than or equal to 0.1 mg / m 3 The specific operation steps are as follows: (1) Place the air purifier in a 5m 3 In the sealed room, turn on the purifier to purify the internal space for 8 hours to remove the interfering components; 2. Measure the LiOH aerosol concentration in the sealed room as the background concentration. The specific sampling method is as follows: (1) Place the sampler with the filter membrane into the sealed room after purification, and sample at a flow rate of 30L / min for 60 minutes; (2) Take out the sampler filter membrane, soak it in a beaker containing 20mL of ultrapure water, mark the sample number, and measure the Li content in the solution with a plasma atomic emission spectrometer; (3) Take out the air purifier, place the carbon dioxide absorption device into the sealed room, place the LiOH tank into the device, and cover the device. Cover the air outlet of the device with an airtight bag and seal it well. Arrange the sampler near the small opening of the sealed bag according to standard requirements; (4) Start the device and sample at a flow rate of 30L / min for 10 minutes; (5) Close the device. Take out the filter membrane of the sampler, immerse it in a beaker containing 20 mL of ultrapure water, mark the sample number, and measure the Li content in the solution using a plasma atomic emission spectrometer; (6) Calculate the dust rate of the lithium hydroxide can filled with the spherical lithium hydroxide reagent sample. The test results show that the dust rate of the canned spherical lithium hydroxide is less than 0.001 mg / m 3 This shows that canned spherical lithium hydroxide is not easy to produce dust, and there will be no problems such as powder falling and choking.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing spherical lithium hydroxide, characterized in that: The following steps are involved: 1) dissolving the coating powder in water to obtain a coating powder solution; 2) adding lithium hydroxide monohydrate powder to a granulator, starting the equipment, and then adding the coating powder solution by intermittent spraying to perform granulation; the intermittent spraying method of adding water is as follows: during the granulation process, the material is uniformly sprayed every 1-5 minutes for 5-40 seconds; 3) continuing to add an appropriate amount of lithium hydroxide monohydrate powder to the granulator, and then adding the coating powder solution by intermittent spraying to coat the lithium hydroxide monohydrate powder on the surface of the sphere; the intermittent spraying method of adding water is specifically: uniformly spraying the material every 1-5 minutes for 5-40 seconds; 4) Repeat step 3) until the designed amount of lithium hydroxide monohydrate powder is reached; 5) Screening out spherical lithium hydroxide with a particle size of 2-4 mm; 6) Drying the spherical lithium hydroxide with a particle size of 2-4 mm to obtain.

2. The method for preparing spherical lithium hydroxide according to claim 1, characterized in that: In step 1), the coating powder is selected from at least one of hydroxypropyl cellulose, hydroxypropyl methyl cellulose, acrylic resin IV, polyvinyl pyrrolidone, and polyvinyl acetal diethylamine acetic acid; And / or, in step 1), the concentration of the coating powder solution is 1%-15wt%.

3. The method for preparing spherical lithium hydroxide according to claim 1, characterized in that: In step 2) and step 3), the particle size of the lithium hydroxide monohydrate is 5-80 microns, preferably 5-30 microns.

4. The method for preparing spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 2), the granulator is a round pot granulator or a disc granulator.

5. The method for preparing spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 2), the weight of lithium hydroxide monohydrate powder initially added is 25-50% of the designed amount; And / or, in step 3), the weight of lithium hydroxide monohydrate powder added each time is 5-15% of the designed amount.

6. The method for preparing spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 2), the amount of water added is 5-15% of the mass of the lithium hydroxide monohydrate powder added in step 2).

7. The method for preparing spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 3), the amount of water added is 5-15% of the mass of the lithium hydroxide monohydrate powder added in step 3).

8. The method for preparing spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 6), the drying temperature is 100 to 180° C. and the drying time is 2 to 15 hours.

9. A spherical lithium hydroxide, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the spherical lithium hydroxide according to claim 9 in adsorbing carbon dioxide.

Citation Information

Patent Citations

  • Lithium hydroxide monohydrate and preparation method thereof

    CN102020294A

  • Preparation process and application of lithium hydroxide spherical absorbent

    CN114749146A

  • High-strength carbon dioxide absorbent particle and preparation method thereof

    CN118320608A

  • Spheritcal granule and its production

    JP1994157353A