Novel spherical lithium hydroxide and preparation method and application thereof

The granulation of lithium hydroxide monohydrate into spherical form addresses dust irritation and cost issues, providing efficient carbon dioxide absorption and low production costs, suitable for confined spaces.

CN119059538APending Publication Date: 2024-12-03THE 718TH RES INST OF CHINA STATE SHIPBUILDING CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410956433.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing lithium hydroxide absorbents used in confined spaces cause dust irritation and have high production costs, necessitating a low-cost method to produce dust-free, high-strength spherical lithium hydroxide with enhanced carbon dioxide absorption efficiency.

Method used

A method involving the granulation of lithium hydroxide monohydrate powder using intermittent water spraying and controlled particle sizes to form spherical lithium hydroxide, followed by screening and drying, ensuring high strength and absorption efficiency.

Benefits of technology

The method produces spherical lithium hydroxide with high carbon dioxide absorption performance, low dust generation, and cost-effectiveness, suitable for mass production and reuse, maintaining a comfortable environment in confined spaces.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of closed space atmospheric environment control, and particularly relates to novel spherical lithium hydroxide as well as a preparation method and application thereof. The preparation method comprises the following steps: adding lithium hydroxide monohydrate powder into a granulator, starting equipment, adding water in an intermittent spraying manner, and granulating; 2) continuing to add a proper amount of lithium hydroxide monohydrate powder into the granulator, then adding water in an intermittent spraying manner, and coating the surface of the sphere with the lithium hydroxide monohydrate powder; (3) repeating the step (2) until the designed dosage of the lithium hydroxide monohydrate powder is reached; (4) screening spherical lithium hydroxide with the particle size of 2-4mm; and 5) drying the spherical lithium hydroxide with the particle size of 2-4mm to obtain the spherical lithium hydroxide. The preparation method is simple and feasible, no waste is generated in the whole process, the cost is low, and the prepared spherical lithium hydroxide has high strength and high carbon dioxide absorption efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of air environment control in confined spaces, and specifically relates to a novel spherical lithium hydroxide and a preparation method and application thereof. Background Art

[0002] As we all know, the control of the atmospheric environment in confined spaces such as space stations, spacecraft, submarines, personal submersibles, mobile lifeboats in coal mines, and emergency refuge chambers is a basic condition for ensuring the safety of personnel life, and the removal of carbon dioxide in confined spaces is of paramount importance. For a long time, relevant departments such as aerospace and navigation in many countries have studied carbon dioxide removal technology in detail. At present, the methods for removing carbon dioxide in confined spaces mainly include lithium hydroxide absorption method, soda lime absorption method, monohydroxyethylamine liquid adsorption method, solid amine adsorption method, alkali metal peroxide absorption method, etc. Among them, lithium hydroxide, as a carbon dioxide absorbent, has the absolute advantages of light weight and high absorption efficiency, but because lithium hydroxide dust has a large irritation to the human respiratory tract, which is particularly obvious in confined spaces, researchers still need to develop absorbents with appropriate structures to reduce the dust rate of lithium hydroxide, effectively prevent the dust of the absorbent, and improve the comfort of personnel in confined spaces. In addition, due to the high cost of lithium hydroxide raw materials, it is necessary to give priority to the process method of preparing lithium hydroxide absorbent at low cost. Summary of the invention

[0003] The purpose of the present invention is to provide a new type of spherical lithium hydroxide and a preparation method and application thereof. The preparation method uses lithium hydroxide monohydrate as a raw material and pure water as a medium. The fine powder of lithium hydroxide monohydrate is bonded layer by layer to form spherical lithium hydroxide by rolling. The preparation method is simple and feasible with low cost. The prepared spherical lithium hydroxide has high strength and high carbon dioxide absorption efficiency.

[0004] Specifically, the present invention provides the following technical solutions:

[0005] A novel method for preparing spherical lithium hydroxide comprises the following steps:

[0006] 1) adding lithium hydroxide monohydrate powder to a granulator, starting the equipment, and then adding water by intermittent spraying to perform granulation; the intermittent spraying method of adding water is as follows: during the granulation process, the material is uniformly sprayed every 1-5 minutes for 5-40 seconds;

[0007] 2) continuing to add an appropriate amount of lithium hydroxide monohydrate powder to the granulator, and then adding water by intermittent spraying to coat the surface of the sphere with the lithium hydroxide monohydrate powder; the intermittent spraying method of adding water is specifically: uniformly spraying the material every 1-5 minutes for 5-40 seconds;

[0008] 3) Repeat step 2) until the designed amount of lithium hydroxide monohydrate powder is reached;

[0009] 4) Screening out spherical lithium hydroxide with a particle size of 2-4 mm;

[0010] 5) Drying the spherical lithium hydroxide with a particle size of 2-4 mm to obtain.

[0011] Preferably, in step 1) and step 2), the particle size of the lithium hydroxide monohydrate is 5-80 microns, more preferably 5-30 microns. Studies have found that using lithium hydroxide monohydrate in the above particle size range as a raw material, the surface of the prepared spherical lithium hydroxide is more rounded, which is conducive to enhancing the strength of the spherical lithium hydroxide.

[0012] Preferably, in step 1), the granulator is a round pan granulator or a disc granulator.

[0013] Preferably, in step 1), the weight of the lithium hydroxide monohydrate powder initially added is 25-50% of the designed amount.

[0014] Preferably, in step 2), the weight of lithium hydroxide monohydrate powder added each time is 2-15% of the designed amount.

[0015] The present invention achieves effective control over the particle size of the prepared spherical lithium hydroxide by limiting the initial addition amount and the subsequent single addition amount of lithium hydroxide monohydrate powder, as well as the method of adding water, and can ensure that the proportion of 2-4 mm spherical lithium hydroxide produced in a single production reaches between 70% and 90%.

[0016] Preferably, in step 1), the total amount of water added is 5-15% of the mass of the lithium hydroxide monohydrate powder added in step 1).

[0017] Preferably, in step 2), the total amount of water added is 5-15% of the mass of the lithium hydroxide monohydrate powder added in step 2).

[0018] In step 1) and step 2), if the amount of water added exceeds 15% based on the mass of lithium hydroxide monohydrate powder, a large amount of powder in the equipment sticks to the pot, resulting in a low ball formation rate, and the spherical lithium hydroxide is prone to breakage during the operation of the equipment; if the amount of water added is less than 5%, there is a large amount of lithium hydroxide powder in the equipment, which cannot participate in the balling process, which also results in a low ball formation rate.

[0019] Preferably, in step 4), the spherical lithium hydroxide with a particle size greater than 4 mm is ground and mixed with the spherical lithium hydroxide with a particle size less than 2 mm, and the mixture is returned to step 1) for granulation.

[0020] Preferably, in step 5), the drying temperature is 100-180° C. and the drying time is 2-15 hours.

[0021] More preferably, the drying temperature is 130-160° C. and the drying time is 9-12 hours.

[0022] The present invention also provides a novel spherical lithium hydroxide, which is prepared by the above-mentioned preparation method.

[0023] The present invention also provides application of the novel spherical lithium hydroxide in adsorbing carbon dioxide.

[0024] The beneficial effects of the present invention are at least:

[0025] 1) The present invention provides a novel method for preparing spherical lithium hydroxide, which has a simple preparation process, high efficiency, low cost, and no waste generated during the preparation process, thereby achieving efficient utilization of high-value lithium hydroxide materials and reducing the impact of strongly alkaline lithium hydroxide powder on the environment;

[0026] 2) The novel method for preparing spherical lithium hydroxide provided by the present invention uses pure water as a medium, has low raw material cost, is harmless to the environment, has high process stability, and does not pollute the lithium hydroxide raw material, thereby ensuring that the lithium hydroxide powder can be reused, and can be recycled and reused after being converted into lithium carbonate after absorbing carbon dioxide;

[0027] 3) The present invention provides a novel method for preparing spherical lithium hydroxide, which forms spherical lithium hydroxide by rolling lithium hydroxide monohydrate fine powder layer by layer, thereby ensuring that the spherical lithium hydroxide has high strength and will not fall off and generate lithium hydroxide dust;

[0028] 4) The present invention provides a novel method for preparing spherical lithium hydroxide. The water content of lithium hydroxide monohydrate powder exceeds 43%. The water content of the wet ball of the spherical lithium hydroxide is further increased by rolling the ball with water as the medium. When the wet ball is dried, a large number of gas channels will be left in the spherical lithium hydroxide after the water evaporates. This will greatly increase the contact area of ​​the spherical lithium hydroxide inside the reaction with carbon dioxide, and greatly improve the carbon dioxide absorption performance of the spherical lithium hydroxide.

[0029] 5) The present invention provides a novel method for preparing spherical lithium hydroxide. The spherical lithium hydroxide product obtained has a high packing density, occupies a small volume, and the gaps between different small balls are evenly distributed, and there will be no problem of local gas blockage and short circuit that reduces the carbon dioxide absorption performance. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention is described clearly and completely below. The following embodiments are used to illustrate the present invention, but are not used to limit the scope of the present invention. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in the field or the product instructions are used.

[0031] In the following examples, the industrial-grade lithium hydroxide monohydrate powder used was sourced from Sichuan Yahua Lithium Technology Co., Ltd.

[0032] In the following embodiments, the round pot granulator used is from: Zhengzhou Rongkai Machinery Equipment Co., Ltd., model 100, and in working state, the speed is controlled to be 10-40r / min, and the inclination angle is controlled within the range of 20-35 degrees.

[0033] Example 1

[0034] (1) 10 kg of industrial-grade lithium hydroxide monohydrate powder with a particle size of 5-30 μm was added to a round pot granulator, the equipment was started, and pure water was sprayed onto the material in the equipment by intermittent spraying. The material was evenly sprayed every 5 minutes for 30 seconds, and the final amount of water added was controlled to be 1.5 kg, so that all the powder was moistened and balled into a sphere;

[0035] (2) adding 1 kg of lithium hydroxide monohydrate powder to the round pot granulator again, and spraying pure water onto the material in the equipment by intermittent spraying, spraying the material evenly for 10 seconds every 2 minutes, and finally controlling the amount of water added to 150 g;

[0036] (3) Repeat step 2) until the total amount of lithium hydroxide monohydrate powder added reaches 20 kg (Note: after the last addition of 1 kg of lithium hydroxide monohydrate powder, 150 g of pure water must continue to be sprayed in an intermittent spraying manner);

[0037] (4) Using a vibrating screen machine with a sieve size of 2 mm and 4 mm, sieving out spherical lithium hydroxide with a particle size of 2-4 mm, and grinding the spherical lithium hydroxide with a particle size greater than 4 mm, mixing it with the spherical lithium hydroxide powder with a particle size less than 2 mm and retaining it, which can be directly used for the next pot of lithium hydroxide pelletizing;

[0038] (5) The screened spherical lithium hydroxide with a size of 2-4 mm is transferred to a forced air oven and dried at 100° C. for 15 hours. After drying, the water content of the spherical lithium hydroxide is detected to be less than 0.5%. The prepared spherical lithium hydroxide is then vacuum packaged.

[0039] Example 2

[0040] (1) 15 kg of industrial-grade lithium hydroxide monohydrate powder with a particle size of 5-80 μm was added to a round pot granulator, the equipment was started, and pure water was sprayed onto the material in the equipment by intermittent spraying. The material was evenly sprayed every 4 minutes for 40 seconds, and the final amount of water added was controlled to be 1.5 kg, so that all the powder was moistened and balled into a ball;

[0041] (2) Add 2 kg of lithium hydroxide monohydrate powder to the round pot granulator again, and spray pure water onto the material in the equipment by intermittent spraying. Spray the material evenly every 1 min for 40 s, and finally control the amount of water added to 200 g;

[0042] (3) Repeat step 2) until the total amount of lithium hydroxide monohydrate powder added reaches 30 kg (Note: after the last addition of 1 kg of lithium hydroxide monohydrate powder, 100 g of pure water still needs to be sprayed in an intermittent spraying manner);

[0043] (4) Using a vibrating screen machine with a sieve size of 2 mm and 4 mm, sieving out spherical lithium hydroxide with a particle size of 2-4 mm, and grinding the spherical lithium hydroxide with a particle size greater than 4 mm, mixing it with the spherical lithium hydroxide powder with a particle size less than 2 mm and retaining it, which can be directly used for the next pot of lithium hydroxide pelletizing;

[0044] (5) The screened spherical lithium hydroxide with a size of 2-4 mm is transferred to a forced air oven and dried at 150° C. for 8 hours. After drying, the water content of the spherical lithium hydroxide is detected to be less than 0.5%. The prepared spherical lithium hydroxide is then vacuum packaged.

[0045] Example 3

[0046] (1) 5 kg of industrial-grade lithium hydroxide monohydrate powder with a particle size of 5-80 μm was added to a round pot granulator, the equipment was started, and pure water was sprayed onto the material in the equipment by intermittent spraying. The material was evenly sprayed every 1 minute for 5 seconds, and the final amount of water added was controlled to be 250 g, so that all the powder was moistened and balled into a sphere;

[0047] (2) Add 1 kg of lithium hydroxide monohydrate powder to the round pot granulator again, and spray pure water onto the material in the equipment by intermittent spraying. Spray the material evenly for 10 seconds every 2 minutes, and finally control the amount of water added to 50 g;

[0048] (3) Repeat step 2) until the total amount of lithium hydroxide monohydrate powder added reaches 20 kg (Note: after the last addition of 1 kg of lithium hydroxide monohydrate powder, 50 g of pure water must continue to be sprayed in an intermittent spraying manner);

[0049] (4) Using a vibrating screen machine with a sieve size of 2 mm and 4 mm, sieving out spherical lithium hydroxide with a particle size of 2-4 mm, and grinding the spherical lithium hydroxide with a particle size greater than 4 mm, mixing it with the spherical lithium hydroxide powder with a particle size less than 2 mm and retaining it, which can be directly used for the next pot of lithium hydroxide pelletizing;

[0050] (5) The screened spherical lithium hydroxide with a size of 2-4 mm is transferred to a forced air oven and dried at 180° C. for 2 hours. After drying, the water content of the spherical lithium hydroxide is detected to be less than 0.5%. The prepared spherical lithium hydroxide is then vacuum packaged.

[0051] The spherical lithium hydroxide prepared by the method of the present invention has excellent carbon dioxide absorption performance, high absorption efficiency, long effective absorption time, round and regular particle size, high stacking density and high particle strength, is not easy to generate dust during transportation and use, and is beneficial to improving the comfort of users; at the same time, the manufacturing cost of the spherical lithium hydroxide is low and can be mass-produced.

[0052] Comparative Example 1

[0053] Compared with Example 1, the only difference is that the particle size of the lithium hydroxide monohydrate raw material is 200-500 microns.

[0054] Comparative Example 1: The pelletization was carried out according to the steps and methods in Example 1. It was found that when the raw material particle size was too large, the powder was difficult to agglomerate into pellets, the pelletization ratio was too low, and the surface of the lithium hydroxide after pelletization was rough and the particle strength was low.

[0055] Comparative Example 2

[0056] Compared with Example 2, the only difference is that the amount of water added in step 1) and step 2) is 20% of the mass of the lithium hydroxide monohydrate powder added in the step.

[0057] The results showed that a large amount of powder in the equipment stuck to the pot, resulting in a low ball formation rate, and the spherical lithium hydroxide was prone to breakage during the operation of the equipment.

[0058] Comparative Example 3

[0059] Compared with Example 2, the only difference is that the amount of water added in step 1) and step 2) is 3% of the mass of the lithium hydroxide monohydrate powder added in the step.

[0060] The results showed that there was a large amount of lithium hydroxide powder in the equipment, which could not participate in the pelletizing process, resulting in a low pelletizing rate.

[0061] Comparative Example 4

[0062] Compared with Example 1, the only difference is that the spherical lithium hydroxide with a particle size of less than 2 mm screened out in step (4) is used as the final product for drying in step 5).

[0063] Experimental tests have shown that the carbon dioxide absorption performance of spherical lithium hydroxide with a particle size of less than 2 mm is poor and cannot meet practical applications. This is mainly because the stacking density of spherical lithium hydroxide with a particle size of less than 2 mm is high, and the tight stacking causes the flow of carbon dioxide gas to be blocked and cannot be quickly absorbed.

[0064] Comparative Example 5

[0065] Compared with Example 1, the only difference is that the spherical lithium hydroxide with a particle size greater than 4 mm screened out in step (5) is used as the final product and dried in step 5).

[0066] Experimental tests show that the carbon dioxide absorption performance of spherical lithium hydroxide with a particle size greater than 4 mm is also poor and cannot meet practical applications. This is mainly because the specific surface area of ​​spherical lithium hydroxide with a particle size greater than 4 mm is relatively low. Affected by gas diffusion, the lithium hydroxide in the inner core of the sphere is difficult to participate in the carbon dioxide reaction, resulting in a decrease in the absorption performance.

[0067] Test example

[0068] First, in order to verify the performance of the prepared spherical lithium hydroxide in practical applications, 40m 3 The closed cabin is used to complete the carbon dioxide absorption performance test of spherical lithium hydroxide. 5.3 kg of spherical lithium hydroxide reagent is canned and placed in the corresponding device. When the carbon dioxide concentration in the closed cabin reaches 0.7%, the device is turned on to start the test and record the change of carbon dioxide concentration in the closed cabin with the absorption time. During the test, the ventilation volume of carbon dioxide is controlled at 0.2m 3 / h, and the test is terminated when the carbon dioxide concentration reaches 0.7% again. According to the normal use requirements of the product, it is necessary to ensure that the absorbent controls the carbon dioxide concentration to be lower than 0.7% for an absorption time of more than 10 hours. After multiple closed cabin absorption performance tests, the results show that the effective absorption time of the spherical lithium hydroxide prepared by the present invention exceeds 10 hours, and the absorption time of samples with better performance exceeds 11 hours. Specifically, the absorption times of Examples 1-3 are 11 hours and 3 minutes, 10 hours and 39 minutes, and 10 hours and 21 minutes, respectively.

[0069] Secondly, according to the requirements of GJB 8040-2013 carbon dioxide absorbent specification standard, the carbon dioxide absorption rate of spherical lithium hydroxide was determined. After multiple tests, the results showed that the absorption rates of spherical lithium hydroxide were all higher than 86%. Specifically, the absorption rates of Examples 1-3 were 88.1%, 86.7%, and 86.3%, respectively, which were significantly better than other lithium hydroxide products reported in the literature; by testing the composition of spherical lithium hydroxide, the results showed that the lithium hydroxide content in the spherical lithium hydroxide ranged from 96 to 98.5%.

[0070] Then, the strength of spherical lithium hydroxide is tested, and the test method is as follows: take a spherical lithium hydroxide sample with a beaker, pass a standard sieve with a 2.0mm aperture, weigh 20.00g of the spherical lithium hydroxide sample after sieving with an electronic balance, and put it into a strength test rotating device. A spherical object (about 1cm in diameter) for testing is placed in the device, which is used to collide and rub with the spherical lithium hydroxide under a rotating state to test the strength of the spherical lithium hydroxide particles. Start the strength test rotating device, close it after 15min, pour out the spherical lithium hydroxide sample and pass the standard sieve with a 2.0mm aperture, weigh the weight of the remaining medicine particles on the sieve to calculate the weight change before and after the test, and the strength value is equal to the weight of the remaining medicine particles on the sieve divided by the weight of the spherical lithium hydroxide added. The test results show that the strength values ​​of the spherical lithium hydroxide prepared by Examples 1-3 are all higher than 97.5%. It is proved that this type of spherical lithium hydroxide is not easy to produce lithium hydroxide dust during transportation and use, and can effectively improve the comfort of users.

[0071] Finally, the dust rate of canned spherical lithium hydroxide during use was determined according to actual use conditions, mainly to test whether the LiOH aerosol concentration in the closed cabin is less than or equal to 0.1 mg / m 3 The specific operation steps are as follows: (1) Place the air purifier in a 5m 3In the sealed room, turn on the purifier to purify the internal space for 8 hours to remove the interfering components; 2. Measure the LiOH aerosol concentration in the sealed room as the background concentration. The specific sampling method is as follows: (1) Place the sampler with the filter membrane into the sealed room after purification, and sample at a flow rate of 30L / min for 60 minutes; (2) Take out the sampler filter membrane, soak it in a beaker containing 20mL of ultrapure water, mark the sample number, and measure the Li content in the solution with a plasma atomic emission spectrometer; (3) Take out the air purifier, place the carbon dioxide absorption device into the sealed room, place the LiOH tank into the device, and cover the device. Cover the air outlet of the device with an airtight bag and seal it well. Arrange the sampler near the small opening of the sealed bag according to standard requirements; (4) Start the device and sample at a flow rate of 30L / min for 10 minutes; (5) Close the device. Take out the filter membrane of the sampler, immerse it in a beaker containing 20 mL of ultrapure water, mark the sample number, and measure the Li content in the solution using a plasma atomic emission spectrometer; (6) Calculate the dust rate of the lithium hydroxide can filled with spherical lithium hydroxide reagent samples. The test results show that no Li element was detected during the test, which indicates that canned spherical lithium hydroxide is not easy to generate dust, and there will be no problems of powder falling and choking.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a novel spherical lithium hydroxide, characterized in that: The following steps are involved: 1) adding lithium hydroxide monohydrate powder to a granulator, starting the equipment, and then adding water by intermittent spraying to perform granulation; the intermittent spraying method of adding water is as follows: during the granulation process, the material is uniformly sprayed every 1-5 minutes for 5-40 seconds; 2) continuing to add an appropriate amount of lithium hydroxide monohydrate powder to the granulator, and then adding water by intermittent spraying to coat the surface of the sphere with the lithium hydroxide monohydrate powder; the intermittent spraying method of adding water is specifically: uniformly spraying the material every 1-5 minutes for 5-40 seconds; 3) Repeat step 2) until the designed amount of lithium hydroxide monohydrate powder is reached; 4) Screening out spherical lithium hydroxide with a particle size of 2-4 mm; 5) Drying the spherical lithium hydroxide with a particle size of 2-4 mm to obtain.

2. The method for preparing the novel spherical lithium hydroxide according to claim 1, characterized in that: In step 1) and step 2), the particle size of the lithium hydroxide monohydrate is 5-80 microns, preferably 5-30 microns.

3. The method for preparing the novel spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 1), the granulator is a round pot granulator or a disc granulator.

4. The method for preparing the novel spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 1), the weight of the lithium hydroxide monohydrate powder initially added is 25-50% of the designed amount.

5. The method for preparing the novel spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 2), the weight of lithium hydroxide monohydrate powder added each time is 2-15% of the designed amount.

6. The method for preparing the novel spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 1), the amount of water added is 5-15% of the mass of the lithium hydroxide monohydrate powder added in step 1).

7. The method for preparing the novel spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 2), the amount of water added is 5-15% of the mass of the lithium hydroxide monohydrate powder added in step 2).

8. The method for preparing the novel spherical lithium hydroxide according to claim 1 or 2, characterized in that: In step 5), the drying temperature is 100 to 180° C. and the drying time is 2 to 15 hours.

9. A novel spherical lithium hydroxide, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the novel spherical lithium hydroxide according to claim 9 in adsorbing carbon dioxide.

Citation Information

Patent Citations

  • Method for industrially producing anhydrous lithium hydroxide balls

    CN109553118A

  • Preparation process and application of lithium hydroxide spherical absorbent

    CN114749146A