Ceramic target material for preparing near-infrared light shielding film and preparation method of ceramic target material

By adding molybdenum disulfide and polyethylene additives to the fluorine-doped titanium dioxide nano powder and subjecting to pressing and calcining, the problem of insufficient performance of existing ceramic targets is solved, and high transmittance, strong barrier rate and good quality are achieved Ceramic targets with thermal conductivity and high tensile strength meet the needs of high standards of near-infrared light shielding films.

CN119059809APending Publication Date: 2024-12-03JIANGSUTOGE OPTOELECTRONIC TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411231398.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing ceramic targets used to prepare near-infrared light shielding films, especially fluorine-doped nanotitanium dioxide targets, can not meet the increasingly high standards after film formation. Inadequate thermal conductivity and tensile strength lead to poor performance.

Method used

Molybdenum disulfide additive and polyethylene additive were added to the fluorine-doped titanium dioxide nano powder, and the mold was filled after stirring evenly, and the polyethylene additive was pressed and calcined. The polyethylene additive was removed and polished to obtain a ceramic target with excellent performance.

Benefits of technology

After film formation, the visible light transmittance of ceramic targets is higher than 92% and the near-infrared barrier rate is higher than 51%, the thermal conductivity is higher than 6.20W/(m·K), and the tensile strength is higher than 358.00MPa, which satisfies High-standard near-infrared light shielding film requirements significantly improve the performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059809A_ABST
    Figure CN119059809A_ABST
Patent Text Reader

Abstract

The invention relates to a ceramic target material for preparing a near-infrared light shielding film and a preparation method of the ceramic target material, a molybdenum disulfide additive is added into fluorine-doped titanium dioxide nano powder, the fluorine-doped titanium dioxide nano powder and the molybdenum disulfide additive are uniformly stirred, and the fluorine-doped titanium dioxide nano powder is uniformly covered with the molybdenum disulfide additive; adding a polyethylene additive into the fluorine-doped titanium dioxide nano powder uniformly covered with the molybdenum disulfide additive, and uniformly stirring to obtain a primary product; a mold is filled with the primary product, then the mold is fed into a press machine to be pressed into a blank body, then other steps are combined, the visible light transmittance is higher than 92% and the near-infrared blocking rate is higher than 51% after the ceramic target material obtained through the method forms a film, and the requirement of the ceramic target material needed by the near-infrared light shielding thin film with the higher and higher standard can be met; the thermal conductivity of the obtained ceramic target material is higher than 6.20 W / (m.K), the tensile strength is higher than 358.00 MPa, and the prepared fluorine-doped nano titanium dioxide target material is good in performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic target materials for near-infrared light shielding films, and in particular relates to a ceramic target material for preparing near-infrared light shielding films and a preparation method thereof. Background Art

[0002] Near-infrared light shielding film is a film that can transmit visible light while shielding near-infrared light. It has been widely used in energy conservation and environmental protection, for example, as a glass coating for buildings and cars. The key to the development of near-infrared light shielding film is to prepare near-infrared light shielding materials with excellent performance.

[0003] As for the ceramic target material used to prepare near-infrared light-shielding films, as mentioned in the prior art solution with patent publication number "CN117819967A", a cesium tungsten bronze ceramic target material for preparing near-infrared light-shielding films is prepared. However, from the practical application point of view, the cesium tungsten bronze ceramic target material used to prepare near-infrared light-shielding films is far inferior to the fluorine-doped nano-titanium dioxide target material in terms of visible light transmittance and near-infrared blocking rate after film formation. On the other hand, the visible light transmittance of the fluorine-doped nano-titanium dioxide target material after film formation is generally lower than 90%, and the near-infrared blocking rate is generally lower than 43%, which cannot meet the requirements of ceramic targets required for near-infrared light-shielding films with increasingly higher standards.

[0004] On the other hand, the existing process for producing fluorine-doped nano-titanium dioxide targets is generally still produced by the process with patent publication number "CN104557021A" (only the raw titanium dioxide powder therein is replaced with fluorine-doped titanium dioxide nanopowder). The thermal conductivity of the fluorine-doped nano-titanium dioxide targets obtained in this way is generally lower than 5.00 W / (m·K) and the tensile strength is generally lower than 342.00 MPa. The performance of the fluorine-doped nano-titanium dioxide targets thus produced is poor. Summary of the invention

[0005] In order to solve the shortcomings of the prior art, the present invention proposes a ceramic target material for preparing near-infrared light shielding film and a preparation method thereof, wherein a molybdenum disulfide additive is added to a fluorine-doped titanium dioxide nanopowder, the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive are stirred evenly, so that the fluorine-doped titanium dioxide nanopowder is evenly covered with the molybdenum disulfide additive, and then a polyethylene additive is added to the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stirred evenly, thereby obtaining a primary product; the primary product fills the mold, and then the mold is sent into a press to be pressed into a embryo, and then combined with other steps, the ceramic target material obtained by the present invention has a visible light transmittance higher than 92% and a near-infrared blocking rate higher than 51% after film formation, which can meet the requirements of ceramic targets required for near-infrared light shielding films of increasingly higher standards. The ceramic target material obtained by the present invention has a thermal conductivity higher than 6.20W / (m·K) and a tensile strength higher than 358.00MPa, and the fluorine-doped nano titanium dioxide target material obtained thereby has excellent performance.

[0006] The present invention uses the following technical solutions.

[0007] A method for preparing a ceramic target material for preparing a near-infrared light shielding film comprises the following steps:

[0008] S1: adding a molybdenum disulfide additive into the fluorine-doped titanium dioxide nanopowder, stirring the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive, so that the fluorine-doped titanium dioxide nanopowder is evenly covered with the molybdenum disulfide additive, and then adding a polyethylene additive into the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stirring evenly, thereby obtaining a primary product;

[0009] S2: Fill the mold with the primary product, then put the mold into a press to press it into a blank, and then heat the blank to 350°C to 420°C under an inert gas protective atmosphere to remove the polyethylene additive;

[0010] S3: sending the embryo body after removing the polyethylene additive into a calcining furnace for calcination;

[0011] S4: Polishing the calcined embryo body. The polished embryo body is a ceramic target material used to prepare a near-infrared light shielding film.

[0012] Preferably, the weight ratio of fluorine-doped titanium dioxide nanopowder to molybdenum disulfide additive is 1:

[0013] (0.005~0.03).

[0014] Preferably, the weight ratio of fluorine-doped titanium dioxide nanopowder to polyethylene additive is 1:

[0015] (0.06~0.08).

[0016] Preferably, during the period when the mold is sent into a press to be pressed into an embryonic body: the working pressure of the press is 24Mp to 32Mp, and the pressing time of the press is 0.5min to 1.5min.

[0017] Preferably, the method of sending the embryo body after removing the polyethylene additive into a calcining furnace for calcining comprises:

[0018] The calcining furnace first calcines the embryo after removing the polyethylene additive for 1.5h to 1.7h at a positive pressure of 26Mp to 30Mp and a calcination temperature of 420°C to 480°C;

[0019] The calcining furnace then calcined the embryo body after removing the polyethylene additive for 2.4h to 2.8h under a negative pressure of -12Mp to -16Mp and a calcination temperature of 1320°C to 1460°C, and then cooled to room temperature.

[0020] A ceramic target material for preparing a near-infrared light shielding film, comprising:

[0021] A ceramic target material prepared according to the method for preparing a ceramic target material for preparing a near-infrared light shielding film.

[0022] A device for preparing a ceramic target material for preparing a near-infrared light shielding film, comprising:

[0023] A rectangular carrier, a stabilizing portion, a storage plate and a pressing head of a press;

[0024] The stabilizing part is assembled on one end of the carrier, and the placement plate is arranged in the middle of the top of the stabilizing part; the pressing head is assembled on the other end of the carrier, and one side of the top of the pressing head is located above the stabilizing part and facing the stabilizing part, and is used to press the mold placed on the placement plate.

[0025] Preferably, the pressing head of the press includes a pressing head arranged on a frame of the press.

[0026] Preferably, the stabilizing portion comprises a bottom assembly piece, a sleeve, a top assembly piece, a moving portion, a limiting portion and a stabilizing strip;

[0027] The bottom assembly piece is assembled on the carrier, and the sleeve is assembled on the bottom assembly piece; the top assembly piece is arranged on the sleeve; multiple moving parts are assembled on the bottom assembly piece and are located in the sleeve; each moving part has another moving part that is mirrored with respect to the center line of the sleeve; the top of each moving part is transparent through the top assembly piece, and the top of each moving part is located at a higher point above the storage plate; multiple limiting parts are arranged on the top of each moving part; the stabilizing bar is fixedly connected to the bottom assembly piece, and the stabilizing bar and the storage plate are connected via a tensioning screw.

[0028] Preferably, a plurality of strip-shaped openings 1 are equidistantly provided on the top assembly sheet, each strip-shaped opening 1 is located above a moving part and faces the moving part, and a strip-shaped opening 1 facing the moving part is provided on the top of each moving part.

[0029] The beneficial effect of the present invention is that, compared with the prior art, the present invention aims to add a molybdenum disulfide additive into a fluorine-doped titanium dioxide nanopowder, stir the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive, and evenly cover the fluorine-doped titanium dioxide nanopowder with the molybdenum disulfide additive, and then add a polyethylene additive into the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stir evenly, so as to obtain a primary product; fill a mold with the primary product, and then send the mold into a press to press it into an embryo, and then heat the embryo to 350°C to 42 0℃ to remove the polyethylene additive; sending the embryo body after removing the polyethylene additive into a calcination furnace for calcination; polishing the calcined embryo body, and the polished embryo body is a ceramic target material for preparing near-infrared light shielding film; the ceramic target material obtained by the present invention has a visible light transmittance higher than 92% and a near-infrared blocking rate higher than 51% after film formation, which cannot meet the requirements of ceramic target materials required for near-infrared light shielding films of increasingly higher standards. The ceramic target material obtained by the present invention has a thermal conductivity higher than 6.20W / (m·K) and a tensile strength higher than 358.00MPa, and the fluorine-doped nano-titanium dioxide target material obtained thereby has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is an overall flow chart of the method for preparing a ceramic target material for preparing a near-infrared light shielding film described in the present invention;

[0031] Figure 2 It is a three-dimensional schematic diagram of an apparatus used in the method for preparing a ceramic target material for preparing a near-infrared light shielding film described in the present invention;

[0032] Figure 3 is a side schematic diagram of the stabilizing portion of the present invention;

[0033] Figure 4 is a lateral schematic diagram of the moving part of the present invention;

[0034] Figure 5 is a schematic diagram of the stabilizing strip of the present invention;

[0035] Figure 6 is a cross-sectional view of the stabilizing strip of the present invention;

[0036] Figure 7 is a cross-sectional view of the limiting piece portion of the present invention;

[0037] Figure 8It is a flat schematic diagram of the pressure head portion of the present invention;

[0038] Fig. 9 It is a partial schematic diagram of the pressure head portion of the present invention;

[0039] Fig.10 It is a schematic diagram of the extended limiting piece described in the present invention. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely expressed in combination with the drawings in the embodiments of the present invention. The embodiments expressed in this application are only part of the embodiments of the present invention, not all of them. Based on the spirit of the present invention, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention.

[0041] like Figure 1 As shown, a method for preparing a ceramic target material for preparing a near-infrared light shielding film according to the present invention comprises:

[0042] S1: Adding a molybdenum disulfide additive into fluorine-doped titanium dioxide nanopowder, stirring the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive, allowing the fluorine-doped titanium dioxide nanopowder to be evenly covered with the molybdenum disulfide additive, and then adding a polyethylene additive into the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stirring to obtain a primary product; the fluorine-doped titanium dioxide nanopowder can be the fluorine-doped titanium dioxide nanopowder prepared in the technical solution with patent publication number "CN113149069B".

[0043] In a preferred but non-limiting embodiment of the present invention, the weight ratio of the fluorine-doped titanium dioxide nanopowder to the molybdenum disulfide additive is 1:(0.005-0.03).

[0044] In a preferred but non-limiting embodiment of the present invention, the weight ratio of the fluorine-doped titanium dioxide nanopowder to the polyethylene additive is 1:(0.06-0.08).

[0045] S2: Fill the mold with the primary product, then send the mold into a press to press it into a embryo, and then heat the embryo to 350℃~420℃ under an inert gas protective atmosphere to remove the polyethylene additive; the mold is a matching mold customized according to the shape of the ceramic target material to be constructed for preparing near-infrared light shielding film.

[0046] In a preferred but non-limiting embodiment of the present invention, during the period when the mold is sent into a press to be pressed into an embryo body: the working pressure of the press is 24Mp to 32Mp, and the pressing time of the press is 0.5min to 1.5min.

[0047] S3: sending the embryo body after removing the polyethylene additive into a calcining furnace for calcination;

[0048] In a preferred but non-limiting embodiment of the present invention, the method of sending the embryo body after removing the polyethylene additive into a calcining furnace for calcining comprises:

[0049] The calcining furnace first calcines the embryo after removing the polyethylene additive for 1.5h to 1.7h at a positive pressure of 26Mp to 30Mp and a calcination temperature of 420°C to 480°C;

[0050] The calcining furnace then calcined the embryo body after removing the polyethylene additive for 2.4h to 2.8h under a negative pressure of -12Mp to -16Mp and a calcination temperature of 1320°C to 1460°C, and then cooled to room temperature.

[0051] S4: Polishing the calcined embryo body. The polished embryo body is a ceramic target material used to prepare a near-infrared light shielding film.

[0052] The ceramic target material for preparing a near-infrared light shielding film according to the present invention comprises:

[0053] A ceramic target material prepared according to the method for preparing a ceramic target material for preparing a near-infrared light shielding film.

[0054] The present invention aims to add a molybdenum disulfide additive into a fluorine-doped titanium dioxide nanopowder, stir the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive, and evenly cover the fluorine-doped titanium dioxide nanopowder with the molybdenum disulfide additive, and then add a polyethylene additive into the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stir evenly, so as to obtain a primary product; fill a mold with the primary product, and then send the mold into a press to press it into an embryo, and then heat the embryo to 350°C to 420°C in an inert gas protective atmosphere to remove the polyethylene additive. Adding agent; sending the embryo body after removing the polyethylene additive into a calcination furnace for calcination; polishing the calcined embryo body, and the polished embryo body is a ceramic target material for preparing near-infrared light shielding film; the ceramic target material obtained by the present invention has a visible light transmittance higher than 92% and a near-infrared blocking rate higher than 51% after film formation, which can meet the requirements of ceramic target materials required for near-infrared light shielding films of increasingly higher standards. The ceramic target material obtained by the present invention has a thermal conductivity higher than 6.20W / (m·K) and a tensile strength higher than 358.00MPa, and the fluorine-doped nano-titanium dioxide target material obtained thereby has excellent performance.

[0055] The embodiments of the preparation method of the present invention are as follows:

[0056] Example 1

[0057] A method for preparing a ceramic target material for preparing a near-infrared light shielding film, comprising:

[0058] S1: Adding a molybdenum disulfide additive into fluorine-doped titanium dioxide nanopowder, stirring the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive, allowing the fluorine-doped titanium dioxide nanopowder to be evenly covered with the molybdenum disulfide additive, and then adding a polyethylene additive into the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stirring to obtain a primary product; the fluorine-doped titanium dioxide nanopowder can be the fluorine-doped titanium dioxide nanopowder prepared in the technical solution with patent publication number "CN113149069B".

[0059] The weight ratio of fluorine-doped titanium dioxide nanopowder to molybdenum disulfide additive is 1:0.03.

[0060] The weight ratio of fluorine-doped titanium dioxide nanopowder to polyethylene additive is 1:0.08.

[0061] S2: Fill the mold with the primary product, then send the mold into a press to press it into a blank, and then heat the blank to 350°C under an inert gas protective atmosphere to remove the polyethylene additive; the mold is a matching mold customized according to the shape of the ceramic target material to be constructed for preparing near-infrared light shielding film.

[0062] The mold is sent into a press to be pressed into an embryo body: the working pressure of the press is 24Mp, and the pressing time of the press is 0.5min.

[0063] S3: sending the embryo body after removing the polyethylene additive into a calcining furnace for calcination;

[0064] The method of sending the embryo body after removing the polyethylene additive into the calcining furnace for calcining includes:

[0065] The calcination furnace first calcined the embryo after removing the polyethylene additive for 1.5 hours at a positive pressure of 26Mp and a calcination temperature of 420°C;

[0066] The calcination furnace then calcined the embryo body after removing the polyethylene additive for 2.4 hours at a negative pressure of -16Mp and a calcination temperature of 1320°C, and then cooled to room temperature.

[0067] S4: Polishing the calcined embryo body. The polished embryo body is a ceramic target material used to prepare a near-infrared light shielding film.

[0068] Ceramic targets for preparing near-infrared light shielding films, including:

[0069] The ceramic target is prepared according to the method for preparing a ceramic target for preparing a near-infrared light shielding film described in Example 1.

[0070] Example 2

[0071] A method for preparing a ceramic target material for preparing a near-infrared light shielding film, comprising:

[0072] S1: Adding a molybdenum disulfide additive into fluorine-doped titanium dioxide nanopowder, stirring the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive, allowing the fluorine-doped titanium dioxide nanopowder to be evenly covered with the molybdenum disulfide additive, and then adding a polyethylene additive into the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stirring to obtain a primary product; the fluorine-doped titanium dioxide nanopowder can be the fluorine-doped titanium dioxide nanopowder prepared in the technical solution with patent publication number "CN113149069B".

[0073] The weight ratio of fluorine-doped titanium dioxide nanopowder to molybdenum disulfide additive is 1:0.0175.

[0074] The weight ratio of fluorine-doped titanium dioxide nanopowder to polyethylene additive is 1:0.7.

[0075] S2: Fill the mold with the primary product, then send the mold into a press to press it into a embryo, and then heat the embryo to 350℃~420℃ under an inert gas protective atmosphere to remove the polyethylene additive; the mold is a matching mold customized according to the shape of the ceramic target material to be constructed for preparing near-infrared light shielding film.

[0076] The mold is sent into a press to be pressed into an embryo body: the working pressure of the press is 28Mp, and the pressing time of the press is 1.0min.

[0077] S3: sending the embryo body after removing the polyethylene additive into a calcining furnace for calcination;

[0078] The method of sending the embryo body after removing the polyethylene additive into the calcining furnace for calcining includes:

[0079] The calcination furnace first calcined the embryo after removing the polyethylene additive for 1.6 hours at a positive pressure of 28Mp and a calcination temperature of 450°C;

[0080] The calcination furnace then calcined the embryo body after removing the polyethylene additive for 2.68 hours at a negative pressure of -14Mp and a calcination temperature of 1340°C, and then cooled to room temperature.

[0081] S4: Polishing the calcined embryo body. The polished embryo body is a ceramic target material used to prepare a near-infrared light shielding film.

[0082] Ceramic targets for preparing near-infrared light shielding films, including:

[0083] The ceramic target is prepared according to the method for preparing a ceramic target for preparing a near-infrared light shielding film described in Example 2.

[0084] Example 3

[0085] A method for preparing a ceramic target material for preparing a near-infrared light shielding film, comprising:

[0086] S1: Adding a molybdenum disulfide additive into fluorine-doped titanium dioxide nanopowder, stirring the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive, allowing the fluorine-doped titanium dioxide nanopowder to be evenly covered with the molybdenum disulfide additive, and then adding a polyethylene additive into the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stirring to obtain a primary product; the fluorine-doped titanium dioxide nanopowder can be the fluorine-doped titanium dioxide nanopowder prepared in the technical solution with patent publication number "CN113149069B".

[0087] The weight ratio of fluorine-doped titanium dioxide nanopowder to molybdenum disulfide additive is 1:0.005.

[0088] In a preferred but non-limiting embodiment of the present invention, the weight ratio of the fluorine-doped titanium dioxide nanopowder to the polyethylene additive is 1:0.06.

[0089] S2: Fill the mold with the primary product, then send the mold into a press to press it into a blank, and then heat the blank to 420°C under an inert gas protective atmosphere to remove the polyethylene additive; the mold is a matching mold customized according to the shape of the ceramic target material to be constructed for preparing near-infrared light shielding film.

[0090] The mold is sent into a press to be pressed into an embryo body: the working pressure of the press is 32Mp, and the pressing time of the press is 1.5 minutes.

[0091] S3: sending the embryo body after removing the polyethylene additive into a calcining furnace for calcination;

[0092] The method of sending the embryo body after removing the polyethylene additive into the calcining furnace for calcining includes:

[0093] The calcination furnace first calcined the embryo after removing the polyethylene additive for 1.7 hours at a positive pressure of 30Mp and a calcination temperature of 480°C;

[0094] The calcination furnace then calcined the embryo body after removing the polyethylene additive for 2.8 hours at a negative pressure of -12Mp and a calcination temperature of 1460°C, and then cooled to room temperature.

[0095] S4: Polishing the calcined embryo body. The polished embryo body is a ceramic target material used to prepare a near-infrared light shielding film.

[0096] Ceramic targets for preparing near-infrared light shielding films, including:

[0097] The ceramic target is prepared according to the method for preparing a ceramic target for preparing a near-infrared light shielding film described in Example 3.

[0098] In addition, three control groups were used for reference:

[0099] Control group 1, control group 2 and control group 3 are three groups of cesium tungsten bronze ceramic targets for preparing near-infrared light shielding films, which are prepared under different ratios using the existing technical solution with patent publication number "CN117819967A".

[0100] In this way, the visible light transmittance and near-infrared blocking rate of the target materials obtained in Examples 1 to 3, Control Group 1, Control Group 2 to Control Group 3 after film formation were tested, and the test results in Table 1 were obtained:

[0101] Table 1

[0102] name Visible light transmittance after film formation Near infrared blocking rate after film formation Example 1 93% 53% Example 2 96% 62% Example 3 98% 74% Control group 1 71% 21% Control group 2 83% 33% Control group 3 86% 37%

[0103] It can be seen from Table 1 that the visible light transmittance and near-infrared blocking rate of the target material obtained by the embodiment of the present invention after film formation are significantly higher than the visible light transmittance and near-infrared blocking rate of the control group 1, the control group 2 and the control group 3 using the prior art solution, that is, the visible light transmittance and near-infrared blocking rate of the ceramic target material obtained by the embodiment of the present invention after film formation are higher than 92% and the near-infrared blocking rate is higher than 51%, which can meet the requirements of ceramic target materials required for near-infrared light shielding films of increasingly higher standards, and are significantly improved than the visible light transmittance and near-infrared blocking rate of the target material obtained by the control group 1, the control group 2 and the control group 3 after film formation obtained by the prior art.

[0104] In addition, three additional control groups were used for reference:

[0105] Control group 4, control group 5 and control group 6 are three groups of fluorine-doped nano titanium dioxide targets prepared under different ratios using the existing technical solution with patent publication number "CN104557021A" (only the raw titanium dioxide powder therein is replaced with fluorine-doped titanium dioxide nanopowder).

[0106] In this way, the thermal conductivity and tensile strength of the target materials obtained in Examples 1 to 3, Control Group 4, and Control Group 5 to Control Group 6 were tested respectively, and the test results in Table 2 were obtained:

[0107] Table 2

[0108]

[0109]

[0110] It can be seen from Table 2 that the thermal conductivity and tensile strength of the target material obtained by the embodiment of the present invention are significantly higher than the thermal conductivity and tensile strength of the control group 4, the control group 5 and the control group 6 using the prior art solution, that is, the thermal conductivity of the ceramic target material obtained by the embodiment of the present invention is higher than 6.20W / (m·K) and the tensile strength is higher than 358.00MPa. The fluorine-doped nano-titanium dioxide target material obtained thereby has good performance, which is significantly improved than the thermal conductivity and tensile strength of the target material obtained by the control group 4, the control group 5 and the control group 6 obtained by the prior art.

[0111] In addition, now that the mold is placed on the placement plate of the press, the limiting device must be used to change the position of the mold so that the mold can be accurately placed under the pressure head of the press and the mold can be accurately pressed.

[0112] However, the current mold limit devices for presses are generally only equipped with limit devices on both sides of the mold, and very few limit devices can achieve limit execution on the four sides of the mold. However, there are still defects such as poor mold limit accuracy, insufficient efficiency during press pressing, and incompatibility with molds of different shapes and sizes.

[0113] After improvement, such as Figures 2 to 10 As shown, the device used in the method for preparing a ceramic target material for preparing a near-infrared light shielding film according to the present invention comprises:

[0114] A rectangular carrier 2, a stabilizing portion 3, a storage plate 4 and a pressing head 5 of a press;

[0115] The stabilizing portion 3 is assembled on one end of the carrier 2. The stabilizing portion 3 is detachable and is compatible with different presses. The shape of the stabilizing portion 3 is not restricted. In this application, setting the stabilizing portion 3 to be rod-shaped is just an example; the placement plate 4 is arranged in the middle of the top of the stabilizing portion 3. The placement plate 4 is detachable and is used to place the mold; the pressing head 5 is assembled on the other end of the carrier 2. One side of the top of the pressing head 5 is above the stabilizing portion 3 and faces the stabilizing portion 3, and is used to press the mold placed on the placement plate 4.

[0116] In a preferred but non-limiting embodiment of the present invention, the ram head 5 of the press comprises a ram disposed on a frame of the press.

[0117] In a preferred but non-limiting embodiment of the present invention, the stabilizing portion 3 comprises a bottom assembly piece 32, a sleeve 33, a top assembly piece 34, a moving portion 35, a limiting portion 36 and a stabilizing bar 36;

[0118] The bottom assembly sheet 32 ​​is assembled on the carrier 2, and the sleeve 33 is assembled on the bottom assembly sheet 32 ​​to prevent particulate impurities from mixing into the stabilizing portion 3; the top assembly sheet 34 is arranged on the sleeve 33; a plurality of moving parts 35 are assembled on the bottom assembly sheet 32 ​​and are located in the sleeve 33; each moving part 35 has another moving part 35 which is mirror-imaged with respect to the center line of the sleeve 33; the top of each moving part 35 is provided with the top assembly sheet 34, and the top of each moving part 35 is located at a higher point above the storage plate 4; a plurality of limiting parts 36 are arranged on the top of each moving part 35 to limit and stabilize the mold; the stabilizing bar 36 is fixedly connected to the bottom assembly sheet 32, and the stabilizing bar 36 is connected to the storage plate 4 via a tensioning screw, and is used to transmit the pressing effect suffered by the storage plate 4 during pressing to the bottom assembly sheet 32, so that the top assembly sheet 34 does not produce obvious strain.

[0119] In a preferred but non-limiting embodiment of the present invention, a plurality of strip openings 342 are equidistantly opened on the top mounting sheet 34, each strip opening 342 is located above a moving portion 35 and faces the moving portion 35, and a strip opening 342 facing the moving portion 35 is formed on the top of each moving portion 35.

[0120] In a preferred but non-limiting embodiment of the present invention, the moving part 35 includes a strip guide port 352, a motor 353, a lifting device 354, a lead screw 355 and a guide piece 356;

[0121] A plurality of guide openings 352 are assembled on the bottom assembly plate 32 and are located in the sleeve 33; each guide opening 352 has another guide opening 352 which is arranged in a mirror image with respect to the center line of the bottom assembly plate 32; a plurality of motors 353 are fixedly connected to each guide opening 352 at the end which is farther from the midpoint of the bottom assembly plate 32, the rotating rod of the motor 353 is linked to the lifting and lowering device 354, and the side of the lifting and lowering device 354 close to the guide opening 352 is fixedly connected to the guide opening 352; one end of the lead screw 355 is threadedly connected to the thread opening on the lifting and lowering device 354, and the other end of the lead screw 355 is fixedly connected to the guide plate 356, and the bottom of the guide plate 356 is placed in the guide opening 352 to allow the guide plate 356 to move in the guide opening 352.

[0122] In a preferred but non-limiting embodiment of the present invention, the moving part 35 further includes a second motor 357, a second lifting device 358 and a second screw 359;

[0123] Motor 2 357 is arranged at the top of guide piece 1 356, and motor 2 357 is linked to lifting and lowering device 2 358, and the bottom wall of lifting and lowering device 2 358 is kept parallel to the top wall of guide piece 1 356; lead screw 2 359 is threadedly connected to the threaded mouth on lifting and lowering device 2 358, and lead screw 2 359 is vertically arranged on the top wall of guide piece 1 356; a pair of supporting bars 360 are also provided on the top of guide piece 1 356, and the bottom of the supporting bars 360 is fixedly connected to the top of guide piece 1 356, and the top of the supporting bars 360 is fixedly connected to lifting and lowering device 2 358, so that lead screw 2 359 can move more smoothly in the vertical direction.

[0124] The lifting and lowering device 1 354 and the lifting and lowering device 2 358 can both be micro electric hoists. The micro electric hoists have the characteristics of centralized structure, small occupied area, light weight, etc., and are suitable for installation and use in small areas.

[0125] In a preferred but non-limiting embodiment of the present invention, the limiting portion 36 includes a block-shaped limiting body 362, a limiting piece portion 364 and an inserting portion 365;

[0126] A plurality of limiting bodies 362 are assembled on the top of each lead screw 359, and the top of each lead screw 359 is in a limiting body 362; the limiting sheet 364 is arranged horizontally, one end of the limiting sheet 364 is clamped in the middle of one side wall of the limiting body 362, and the other end of the limiting sheet 364 is close to the storage plate 4; the plug-in part 365 is arranged in the middle of the other side wall of the limiting body 362, one end of the plug-in part 365 is in the limiting body 362 and contacts with the limiting sheet 364, and the other end of the plug-in part 365 is outside the limiting body 362, and the plug-in part 365 and the limiting sheet 364 are arranged facing each other;

[0127] The limiting portion 36 further includes a stabilizing strip 363 and plastic particles 366;

[0128] The stabilizing bar 1 363 is provided through the top of the second screw 359 and the bottom of the limiting body 362, so that the top of the second screw 359 is fixedly connected to the limiting body 362; a plurality of plastic particles 366 are provided on one side of the limiting body 362 close to the placement plate 4, which are used to increase the hindrance effect between the mold; a plurality of plastic particles 366 are also provided on the top wall and the bottom wall of the limiting sheet 364 at the end outside the limiting body 362, which are also used to increase the hindrance effect between the mold and make the mold more stable on the placement plate 4.

[0129] In a preferred but non-limiting embodiment of the present invention, the limiting piece portion 364 includes a limiting piece 3642, an opening 1 3643, a spring 2533, a limiting ball 3645 and an opening 2 3646;

[0130] One end of the limiting piece 3642 is laterally embedded in the limiting body 362, and the other end of the limiting piece 3642 is close to the storage plate 4, and a plurality of plastic particles 366 are arranged on the top wall and the bottom wall of the limiting piece 3642 at the end outside the limiting body 362; an opening 1 3643 is arranged at the end of the limiting piece 3642 in the limiting body 362, a spring 2533 is arranged in the opening 1 3643, one end of the spring 2533 is fixedly connected to the bottom of the opening 1 3643, and the other end of the opening 1 3643 is fixedly connected to the limiting ball 3645, and one end of the limiting ball 3645 is arranged in the opening 1 3643; an opening 2 3646 is also arranged at the end of the limiting piece 3642 outside the limiting body 362, and the opening 2 3646 is used to place instruments such as wrenches and pliers through the limiting piece 3642, which is convenient for maintenance.

[0131] Because multiple limiting plates 3642 are located in the middle of each limiting body 362, when the size of the mold exceeds the storage plate, multiple non-adjacent limiting bodies 362 are located below the limiting plates 3642 and contact the side wall of the mold, and the bottom wall of the limiting plates 3642 contacts the top wall of the mold; another multiple non-adjacent limiting bodies 362 are located above the limiting plates 3642 and contact the side wall of the mold, and the top wall of the limiting plates 3642 contacts the bottom wall of the mold; at this time, multiple limiting plates 3642 are in sequential and staggered contact with the top and bottom walls of the mold, so that the mold does not produce a large strain due to uneven force.

[0132] In a preferred but non-limiting embodiment of the present invention, the plug-in portion 365 includes a second stabilizing bar 3652 and a moving bar 3653;

[0133] One end of the second stabilizing bar 3652 is arranged in the limiting body 362, and the moving bar 3653 can move through the second stabilizing bar 3652. One end of the second stabilizing bar 3652 in the limiting body 362 is provided with a strip-shaped opening 3654, and the strip-shaped opening 3654 contacts the limiting ball 3645. One end of the moving bar 3653 in the second stabilizing bar 3652 contacts the limiting ball 3645. By dragging the moving bar 3653, the limiting ball 3645 can be returned to the opening 1 3643, and the limiting sheet 3642 can be dragged to separate through the limiting body 362.

[0134] In a preferred but non-limiting embodiment of the present invention, the pressure head 5 comprises a third lifting and lowering device 52 (which may be a micro electric hoist), a second guide piece 53, a pressure head 54 and an assembly ring 55;

[0135] The guide piece 2 53 is assembled on the bottom wall of the landing device 3 52 above the storage board 4 and facing one end of the storage board 4. The top of the guide piece 2 53 is linked to the landing device 3 52. The pressure head 54 is fixedly connected to the bottom of the guide piece 2 53. The center line of the pressure head 54 is consistent with the center line of the storage board 4, and the guide piece 2 53 can pull the pressure head 54 to move vertically along the center line of the storage board 4; the assembly ring 55 is fixedly connected to the bottom wall of the landing device 3 52 above the storage board 4 and facing one end of the storage board 4. The guide piece 2 53 is in the assembly ring 55, and the center line of the guide piece 2 53 is consistent with the center line of the assembly ring 55.

[0136] In a preferred but non-limiting embodiment of the present invention, a plurality of ZH5 ultrasonic sensors 56 are also installed in the assembly circle 55; the plurality of ZH5 ultrasonic sensors 56 are equidistantly arranged in the assembly circle 55, and the center line of each ZH5 ultrasonic sensor 56 is in the interval of the top wall of the storage plate 4.

[0137] In a preferred but non-limiting embodiment of the present invention, an extended limiting piece 6 is installed in the second opening 3646 .

[0138] When the limiting plate 3642 cannot limit certain molds, an extended limiting plate 6 can be installed in the second opening 3646 on the limiting plate 3642. One end of the extended limiting plate 6 is connected to the second opening 3646, and the other end of the extended limiting plate 6 is provided with a plurality of plastic particles 366. The other end of the extended limiting plate 6 can limit and stabilize the mold, thereby achieving the limitation and positioning of the mold without changing the existing equipment.

[0139] In this way, after the operator places the mold on the placement plate, the ZH5 ultrasonic sensor 56 starts to work. When there is an error in the placement position of the mold, the distance detected by multiple ZH5 ultrasonic sensors 56 in the error position is higher than the distance detected by other multiple ZH5 ultrasonic sensors 56. At this time, a motor 353 in the opposite direction of the error position is started to pull the limiting body 362 to move beyond the error position until the distances detected by multiple ZH5 ultrasonic sensors 56 are the same, and then the motor 353 is stopped; at this time, the other multiple motors 353 are started to pull the limiting body 362 to move beyond the mold until it contacts the side wall of the mold; the motor 2 357 is started to make the bottom wall of the limiting plate 3642 contact the mold, thereby achieving the limitation and stability of the mold, and the pressing head 5 operates to press the mold successfully.

[0140] When the size of the mold exceeds the storage plate, multiple motors 1 353 that are not adjacent to each other are started first to pull the limiting body 362 to move in the direction of the mold, so that the side of the limiting body 362 below the limiting plate 3642 contacts the mold side wall, and the motor 2 357 is started to make the bottom wall of the limiting plate 3642 contact the top wall of the mold; then, another multiple motors 1 353 that are not adjacent to each other are started to pull the limiting body 362 to move in the direction of the mold, so that the side of the limiting body 362 above the limiting plate 3642 contacts the mold side wall, and the motor 2 357 is started to make the top wall of the limiting plate 3642 contact the bottom wall of the mold; at this time, multiple limiting plates 3642 are alternately contacted with the top wall and bottom wall of the mold in sequence, so that when the mold is limited, the force applied to the mold is balanced, and no large strain will be generated.

[0141] In this way, by providing a plurality of movable limiting parts, the four sides, top wall and bottom wall of the mold can be limited synchronously, which improves the limiting accuracy of the mold and also allows the limiting part to be compatible with more molds of different shapes and sizes; by providing a plurality of detachable limiting bodies and limiting plates, when a limiting body or a limiting plate is damaged, the damaged limiting body or limiting plate can be moved to a position away from the storage plate, and the damaged limiting body and limiting plate can be replaced, thereby improving the maintenance efficiency; by providing a limiting plate part, the top walls and bottom walls of the plurality of limiting plate parts can be clamped on the top wall and bottom wall of the mold in sequence, the mold is firmly clamped by the limiting part in the lateral direction, and the side walls of the limiting body are in firm contact with the side walls of the mold, so that the mold cannot move during pressing, thereby improving the pressing efficiency.

[0142] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents, and any modifications or equivalent replacements that do not deviate from the spirit and scope of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a ceramic target material for preparing a near-infrared light shielding film, characterized in that: include: S1: adding a molybdenum disulfide additive into the fluorine-doped titanium dioxide nanopowder, stirring the fluorine-doped titanium dioxide nanopowder and the molybdenum disulfide additive, so that the fluorine-doped titanium dioxide nanopowder is evenly covered with the molybdenum disulfide additive, and then adding a polyethylene additive into the fluorine-doped titanium dioxide nanopowder evenly covered with the molybdenum disulfide additive and stirring evenly, thereby obtaining a primary product; S2: Fill the mold with the primary product, then put the mold into a press to press it into a blank, and then heat the blank to 350°C to 420°C under an inert gas protective atmosphere to remove the polyethylene additive; S3: sending the embryo body after removing the polyethylene additive into a calcining furnace for calcination; S4: Polishing the calcined embryo body. The polished embryo body is a ceramic target material used to prepare a near-infrared light shielding film.

2. The method for preparing a ceramic target material for preparing a near-infrared light shielding film according to claim 1, characterized in that: The weight ratio of fluorine-doped titanium dioxide nanopowder and molybdenum disulfide additive is 1: (0.005~0.03)。 3. The method for preparing a ceramic target material for preparing a near-infrared light shielding film according to claim 2, characterized in that: The weight ratio of fluorine-doped titanium dioxide nanopowder and polyethylene additive is 1: (0.06~0.08)。 4. The method for preparing a ceramic target material for preparing a near-infrared light shielding film according to claim 3, characterized in that: The mold is sent into a press to be pressed into an embryo body: the working pressure of the press is 24Mp to 32Mp, and the pressing time of the press is 0.5min to 1.5min.

5. The method for preparing a ceramic target material for preparing a near-infrared light shielding film according to claim 4, characterized in that: The method of sending the embryo body after removing the polyethylene additive into the calcining furnace for calcining includes: The calcining furnace first calcines the embryo after removing the polyethylene additive for 1.5h to 1.7h at a positive pressure of 26Mp to 30Mp and a calcination temperature of 420°C to 480°C; The calcining furnace then calcined the embryo body after removing the polyethylene additive for 2.4h to 2.8h under a negative pressure of -12Mp to -16Mp and a calcination temperature of 1320°C to 1460°C, and then cooled to room temperature.

6. A ceramic target material for preparing a near-infrared light shielding film, characterized in that: include: A ceramic target material produced according to the method for producing a ceramic target material for producing a near-infrared light shielding film as claimed in any one of claims 1 to 5.

7. An apparatus for use in the method for preparing a ceramic target material for preparing a near-infrared light shielding film as claimed in any one of claims 1 to 5, comprising: A rectangular carrier, a stabilizing portion, a storage plate and a pressing head of a press; The stabilizing part is assembled on one end of the carrier, and the placement plate is arranged in the middle of the top of the stabilizing part; the pressing head is assembled on the other end of the carrier, and one side of the top of the pressing head is located above the stabilizing part and facing the stabilizing part, and is used to press the mold placed on the placement plate.

8. The device used in the method for preparing a ceramic target material for preparing a near-infrared light shielding film according to claim 7, characterized in that: The pressing head of the press includes a pressing head arranged on a frame of the press.

9. The device used in the method for preparing a ceramic target material for preparing a near-infrared light shielding film according to claim 8, characterized in that: The stabilizing part includes a bottom assembly piece, a sleeve, a top assembly piece, a moving part, a limiting part and a stabilizing strip; The bottom assembly piece is assembled on the carrier, and the sleeve is assembled on the bottom assembly piece; the top assembly piece is arranged on the sleeve; multiple moving parts are assembled on the bottom assembly piece and are located in the sleeve; each moving part has another moving part that is mirrored with respect to the center line of the sleeve; the top of each moving part is transparent through the top assembly piece, and the top of each moving part is located at a higher point above the storage plate; multiple limiting parts are arranged on the top of each moving part; the stabilizing bar is fixedly connected to the bottom assembly piece, and the stabilizing bar and the storage plate are connected via a tensioning screw.

10. The device used in the method for preparing a ceramic target material for preparing a near-infrared light shielding film according to claim 9, characterized in that: A plurality of strip-shaped openings are equidistantly provided on the top assembly sheet, each strip-shaped opening is located above a moving part and faces the moving part, and a strip-shaped opening facing the moving part is provided on the top of each moving part.

Citation Information

Patent Citations

  • A fluorine-doped titanium dioxide nanopowder with both transparency and near-infrared shielding functions

    CN113149069B

  • High-compactness titanium oxide target material and preparation method thereof

    CN104557021A

  • Organic and inorganic compound membrane with light selective adsorbing and anti-ageing functions and preparation method thereof

    CN109517254A

  • Fluorine-doped titanium dioxide nano powder with transparent and near-infrared shielding functions