Preparation method of Al2O3-coated C composite material
Al2O3@C composite material is formed through metal aluminum powder boehm petrochemical and gelling treatment, which solves the problems of poor oxidation resistance and non-wetting of scale graphite, simplifies the process and reduces costs, and improves the wettability and performance of the material.
Patent Information
- Application Number
- CN202411553866.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-04
AI Technical Summary
The poor oxidation resistance and non-wetting properties of scale graphite in existing refractory materials lead to limited application in carbon-containing refractory materials, and the preparation process is complex and costly.
AlOOH solution was prepared through the petrochemical process of metal aluminum powder Boehm, graphite and additives were added to stir, and then gelling agent was added to prepare the precursor gel. Heat treatment was performed under a reducing atmosphere to form an Al2O3@C composite material, simplifying the process and improving the wettability of the material .
The Al2O3@C composite material with good wetting is achieved. The raw materials are easily obtained and non-toxic, and the operation process is simple, which reduces production costs and improves the mechanical properties and corrosion resistance of the material.
Smart Images

Figure CN119059826A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and particularly relates to a method for preparing an Al2O3@C composite material. Background Art
[0002] Flake graphite is a material with high thermal conductivity, non-wetting properties to metal slag and low coefficient of thermal expansion, which can significantly improve the thermal shock and corrosion resistance of carbon-containing refractories. However, the limiting factor for this application is its weak oxidation resistance and non-wetting properties. Due to the hydrophobic nature of graphite, the uniform distribution of graphite flakes is challenging, which reduces the fluidity of the resulting monolithic refractory and requires a large amount of water for laying; therefore, the porosity of the product increases significantly after drying, resulting in a decrease in its mechanical properties and corrosion resistance.
[0003] Among them, the public text "A modified graphite material, its preparation method and application" (CN118515267A) discloses a modified graphite material, its preparation method and application. In the modified graphite material, part of the titanium dioxide particles will stick to the carbon coating layer, and the other part will protrude from the carbon coating layer. Titanium dioxide and the carbon coating layer work synergistically to achieve excellent high-rate performance. This method requires nitrogen protection heating and vacuum drying processes, and the operation process is complicated. At the same time, expensive chemicals such as dioxane are used in the reaction, which is costly.
[0004] The public text "Synthesis Method of Boron-Doped Carbon-Coated Graphite" (CN116375018B) discloses a synthesis method of boron-doped carbon-coated graphite. The chemical reaction of B2H6 and CO2 is used to deposit on the surface of the graphite material in the form of chemical vapor deposition in a vapor deposition furnace to form a boron-doped carbon-coated graphite material. B2H6 reacts with CO2 to generate carbon, BC bonds and H2O to form boron-doped carbon, with the graphite substrate as the inner layer and the outer layer as boron-doped carbon. Boron doping changes the electronic structure state of the carbon layer, improves the charge storage and transfer rate, and optimizes the electrochemical performance. This method requires steps such as vapor deposition and condensation, uses a vapor deposition furnace, has a long operation time, and a complex process.
[0005] The public text "A high thermal conductivity spherical sulfonated polyetheretherketone / graphite core-shell structure filler and its preparation method" (CN110684512A) discloses a high thermal conductivity spherical sulfonated polyetheretherketone / graphite core-shell structure filler and its preparation method. Sulfonated polyetheretherketone is prepared by mixing fluoroketone, sulfonated fluoroketone and hydroquinone and then drying to remove 40-60% of the volume of water, and then using a spherical mold to cut the sulfonated polyetheretherketone to obtain spherical sulfonated polyetheretherketone particles of different particle sizes; finally, the spherical sulfonated polyetheretherketone and micron-sized graphite are electrostatically adsorbed to prepare a high thermal conductivity spherical sulfonated polyetheretherketone / graphite core-shell structure filler with sulfonated polyetheretherketone as the core and micron-sized graphite as the shell. This method requires chemical reagents such as fluoroketone, concentrated sulfuric acid, sulfonated fluoroketone, hydroquinone and potassium carbonate, which is costly and environmentally unfriendly. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a preparation method of an Al2O3@C composite material. The present invention adopts a boehmite process of metal aluminum powder to prepare an AlOOH solution; then graphite and additives are added for stirring, and then a gelling agent is added to prepare a precursor gel, and then a heat treatment is performed under a reducing atmosphere to obtain the Al2O3@C composite material. The raw materials used in the synthesis are easy to obtain, non-toxic, and environmentally friendly; the operation process only includes three steps of water bath, gelling and sintering, the operation process is simple, and the prepared Al2O3@C composite material has good wettability.
[0007] In order to achieve the above object, the technical solution of the present invention is: The preparation method of the Al2O3@C composite material of the present invention is: Step 1: 0.4-2 mol of aluminum powder is stirred and heated in a water bath at 80-100° C. for 0.5-2.5 h to prepare an AlOOH solution (i.e., a boehmite solution), and an AlOOH coating layer is formed around the particles; Step 2: Add a polyvinyl alcohol solution having a concentration of 0.04-0.2 g / ml to the solution obtained in step 1, and continue stirring for 0.2-1 h; Step 3: Add flake graphite powder and additives in sequence and continue stirring for 0.5-2.5 hours; the amount of flake graphite added is 0.4-2 mol, which is consistent with the amount of metallic aluminum powder added in step 1; the amount of additives added is 0.05-0.25 mol; Step 4, adding a gelling agent solution with a concentration of 0.05-0.25 g / ml to prepare a precursor gel; Step 5: calcine the precursor gel at 1100°C-1500°C for 1-5h under reducing atmosphere conditions to prepare an Al2O3 coating layer on the graphite surface, thereby obtaining an Al2O3@C composite material.
[0008] The purity of the metal aluminum powder is greater than 98%, and the particle size is less than or equal to 1 μm.
[0009] The purity of the flake graphite is greater than 98%, and the particle size is less than or equal to 10 μm.
[0010] The additive is one or more of analytical pure ferric nitrate, chemical pure ferric nitrate, and industrial pure ferric nitrate, with a purity of more than 99.9%.
[0011] The gelling agent is one or more of analytical pure borax, chemical pure borax and industrial pure borax, and the purity is greater than 99.9%.
[0012] The invention is applied to the preparation of carbon sources in the field of carbon-containing refractory materials.
[0013] The present invention uses metallic aluminum powder because the metallic aluminum powder will undergo a boehmite process under water bath conditions, so that an AlOOH coating layer will be formed around the particles, and then a boehmite solution will be formed. Under the support of the polyvinyl alcohol solution, these particles with the AlOOH coating layer are fixed on the graphite surface through a gelation reaction; at the same time, under reducing atmosphere conditions, a certain CO partial pressure is formed along with the CO formed during the decomposition and addition of boehmite; according to the thermodynamic conditions of the Al-OC system, the regulation of the O2 and CO partial pressures in the environment is conducive to the formation of Al2O3.
[0014] The present invention utilizes the boehmite process to prepare an Al2O3 coating layer on the graphite surface, and regulates the reactivity of Al2O3 by regulating the boehmite process and the amount of additives added. The surface of the newly formed particles is in a metastable state and can react with gases in the environment. The specific surface area of the newly formed particles is relatively increased, and the activity is improved, thereby achieving the integrity of the coating layer.
[0015] In addition, in carbon-containing amorphous refractory materials, poor wettability of graphite will lead to uneven dispersion of graphite therein, which will lead to uneven distribution of thermal stress in the product and cause cracks. The wetting angle of the present invention is 10-40°, which improves the bonding ability of the graphite interface with water.
[0016] The beneficial effects of the present invention are as follows: the present invention carries out a boehmite process on metal aluminum powder under water bath conditions, then adds graphite, polyvinyl alcohol solution and additives and stirs, and prepares a precursor through a gelling agent; the precursor is placed in a reducing atmosphere for heat treatment to obtain an Al2O3@C composite material; the raw materials used in the present invention are easily available, non-toxic, and environmentally friendly; the operation process only includes three steps of water bath, gelling and sintering; the operation process is simple, and the prepared Al2O3@C composite material has good wettability. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1This is the SEM photo of the Al2O3@C composite material prepared in Example 1. DETAILED DESCRIPTION
[0018] The present invention is further described in detail below in conjunction with specific embodiments. An Al2O3@C composite material and a preparation method thereof provided in an embodiment of the present invention, wherein the purity of the metal aluminum powder is greater than 98%, and the particle size is ≤1μm; the purity of the flake graphite is greater than 98%, and the particle size is ≤10μm; 0.4~2mol of the metal aluminum powder is stirred and heated in a water bath at 80~100℃ for 0.5~2.5h to prepare an AlOOH solution; then a polyvinyl alcohol solution with a concentration of 0.04~0.2g / ml is added to the boehmite solution, and stirring is continued for 0.2~1h; then flake graphite powder and additives are added in sequence and stirring is continued for 0.5~2.5h; finally, a gelling agent solution with a concentration of 0.05~0.25g / ml is added to prepare a precursor gel, and the precursor gel is calcined at 1100℃~1500℃ for 1~5h under reducing atmosphere conditions to obtain an Al2O3@C composite material.
[0019] Embodiment 1:
[0020] Step 1: 0.4 mol of aluminum powder was stirred and heated in a water bath at 80°C for 0.5 h to prepare an AlOOH solution (i.e., a boehmite solution); Step 2: Add 0.04 g / ml polyvinyl alcohol solution to the solution obtained in step 1, and continue stirring for 0.2 h; Step 3: Add flake graphite powder and analytical pure ferric nitrate in sequence and continue stirring for 0.5h; the amount of flake graphite added is 0.4mol; the amount of analytical pure ferric nitrate added is 0.05mol; Step 4: adding a 0.05 g / ml chemically pure borax solution to prepare a precursor gel; Step 5: calcine the precursor gel at 1100°C for 1 hour under reducing atmosphere to prepare an Al2O3 coating layer on the graphite surface, thereby obtaining an Al2O3@C composite material with a wetting angle of 25°~40°.
[0021] Embodiment 2:
[0022] Step 1: Stir and heat 1 mol of aluminum powder in a water bath at 85°C for 1 hour to prepare an AlOOH solution (i.e., a boehmite solution); Step 2: Add 0.1 g / ml polyvinyl alcohol solution to the solution obtained in step 1, and continue stirring for 0.5 h; Step 3: Add flake graphite powder and analytical pure ferric nitrate in sequence and continue stirring for 1 hour; the amount of flake graphite added is 1 mol; the amount of analytical pure ferric nitrate added is 0.1 mol; Step 4, adding 0.1 g / ml analytical pure borax solution to prepare a precursor gel; Step 5: calcine the precursor gel at 1200°C for 3h in a reducing atmosphere to prepare an Al2O3 coating layer on the graphite surface, thereby obtaining an Al2O3@C composite material with a wetting angle of 20°~35°.
[0023] Embodiment 3:
[0024] Step 1: Stir and heat 1.5 mol of aluminum powder in a water bath at 90°C for 1.5 h to prepare an AlOOH solution (i.e., a boehmite solution); Step 2: Add 0.15 g / ml polyvinyl alcohol solution to the solution obtained in step 1, and continue stirring for 0.8 h; Step 3: Add flake graphite powder and industrial pure ferric nitrate in sequence and continue stirring for 1.5 hours; the amount of flake graphite added is 1.5 mol; the amount of industrial pure ferric nitrate added is 0.2 mol; Step 4: Add 0.15 g / ml industrial pure borax solution to prepare a precursor gel; Step 5: calcine the precursor gel at 1300°C for 4h under reducing atmosphere to prepare an Al2O3 coating layer on the graphite surface, thereby obtaining an Al2O3@C composite material with a wetting angle of 15°~30°.
[0025] Embodiment 4:
[0026] Step 1: 2 mol of aluminum powder was stirred and heated in a water bath at 100° C. for 2.5 h to prepare an AlOOH solution (i.e., a boehmite solution); Step 2: Add 0.2 g / ml polyvinyl alcohol solution to the solution obtained in step 1 and continue stirring for 1 hour; Step 3: Add flake graphite powder and chemically pure ferric nitrate in sequence and continue stirring for 2.5 hours; the amount of flake graphite added is 2 mol; the amount of chemically pure ferric nitrate added is 0.25 mol; Step 4: Add 0.25 g / ml chemically pure borax solution to prepare a precursor gel; Step 5: calcine the precursor gel at 1500°C for 5h in a reducing atmosphere to prepare an Al2O3 coating layer on the graphite surface, thereby obtaining an Al2O3@C composite material; the wetting angle of the composite material is 10°~25°.
[0027] This preparation method has the following advantages: the raw materials are non-toxic, harmless, and easily available, and the production cost is low; the preparation process only requires a water bath, gelation, and heat treatment processes, and the process is simple.
[0028] The parts of the present invention that are not described in detail are prior art. The above embodiments will help relevant persons in the art to further understand the present invention, but do not limit the present invention in any form. Within the scope of the present invention defined by the attached claims, various changes in form, details or equivalents made using the present invention are all within the protection scope of the present invention.
Claims
1. A kind of Al 2 O 3 @C Preparation method of composite material, Features: Step 1: 0.4-2 mol of aluminum powder is stirred and heated in a water bath at 80-100° C. for 0.5-2.5 h to prepare an AlOOH solution; an AlOOH coating layer is formed around the particles; Step 2: Add a polyvinyl alcohol solution having a concentration of 0.04-0.2 g / ml to the solution obtained in step 1, and continue stirring for 0.2-1 h; Step 3: Add flake graphite powder and additives in sequence and continue stirring for 0.5-2.5 hours; the amount of flake graphite added is 0.4-2 mol, which is consistent with the amount of metallic aluminum powder added in step 1; the amount of additives added is 0.05-0.25 mol; Step 4, adding a gelling agent solution with a concentration of 0.05-0.25 g / ml to prepare a precursor gel; Step 5: calcine the precursor gel at 1100℃~1500℃ for 1~5h in a reducing atmosphere to prepare Al on the graphite surface. 2 O 3 The encapsulation layer is Al 2 O 3 @C composite material, wetting angle is 10-40°.
2. A kind of Al according to claim 1 2 O 3 @C Preparation method of composite material, Features: The purity of the metal aluminum powder is >98% and the particle size is ≤1μm.
3. A kind of Al according to claim 1 2 O 3 @C Preparation method of composite material, Features: The purity of flake graphite is >98% and the particle size is ≤10μm.
4. A kind of Al according to claim 1 2 O 3 @C Preparation method of composite material, Features: The additive is one or more of analytical pure ferric nitrate, chemical pure ferric nitrate and industrial pure ferric nitrate, with a purity of more than 99.9%.
5. A kind of Al according to claim 1 2 O 3 @C Preparation method of composite material, Features: The gelling agent is one or more of analytical pure borax, chemical pure borax and industrial pure borax, with a purity of more than 99.9%.
Citation Information
Patent Citations
Method for preparing hydrophilic graphite / oxide composite powder
CN101186456A
Preparation method of alpha-Al2O3 nanoparticles
CN109516483A
Preparation method of high-wettability graphite-based composite powder
CN115215654A
Lightweight carbon-based multiphase microsphere and preparation method thereof
CN118047620A
Alumina coated graphite, method for manufacturing the same, and refractory with low thermal conductivity
KR1020110077346A
Cited By
Preparation method of multi-ceramic combined lightweight magnesia-carbon composite material
CN120398517A
Preparation method of multi-ceramic combined light magnesium carbonaceous composite material
CN120398517B