Self-cleaning concrete surface strengthening material and preparation method thereof

Through a microsphere emulsion with a three-layer structure in water (W1/O/W2), the photosensitive trifluoromethylbenzene silanepyrazo azo compound is used to achieve photo-triggered emulsion decomposition, which solves the complex process in the existing technology and The problem of restricted release significantly improves concrete surface performance and durability, and is suitable for high-end buildings and landscape projects.

CN119059840APending Publication Date: 2024-12-03JIANGSU CHINA RAILWAY ARIT NEW MATEIRALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411125764.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The preparation process of existing concrete surface reinforcement materials is complex and is not suitable for large-scale production. The release of effective reinforcement components is limited, resulting in insufficient penetration depth and single function, insufficient long-term and durability, which cannot meet the needs of high-end buildings and landscape engineering.

Method used

Microsphere-like configuration emulsion with a three-layer structure of water-in-water (W1/O/W2) is adopted. The internal aqueous phase contains fluorosilicates, nanooxides, silicates and cosolvents, and the intermediate oil phase is photosensitive three Fluoromethylbenzene silanepyrazo azo compound, the outer aqueous phase contains permeability agent and dispersant, is prepared by high-pressure homogenizer and microfluidic emulsification technology, and light-triggered emulsification under light conditions to simplify construction operations.

Benefits of technology

The protection and controlled release of active ingredients are achieved, the surface performance of concrete is improved, the penetration depth and the strength of crystallized products are enhanced, the needs of high-end buildings and landscape engineering are met, and the preparation process and construction process are simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004996353040000031
    Figure BDA0004996353040000031
  • Figure BDA0004996353040000061
    Figure BDA0004996353040000061
  • Figure BDA0004996353040000071
    Figure BDA0004996353040000071
Patent Text Reader

Abstract

The invention discloses a self-cleaning concrete surface strengthening material and a preparation method thereof. The strengthening material is a microspheric configuration emulsion with a water-in-oil-in-water three-layer structure. An internal water phase is a mixed solution composed of fluosilicate, nano oxide, silicate, sulfate and a cosolvent; the oil phase is a trifluoromethyl phenylsilane pyrazole azo compound; and the outer water phase consists of a penetration enhancer and a dispersing agent. The preparation method comprises the following steps: mixing the reinforcing component of the internal water phase, the azoic compound of the oil phase and the emulsifier, and shearing and emulsifying through a high-pressure homogenizer to obtain a primary W1 / O emulsion; and carrying out secondary emulsification on the primary emulsion and the outer-layer water phase through a micro-fluidic emulsification technology to obtain a dual W1 / O / W2 emulsion, namely the self-cleaning type concrete surface strengthening material. The reinforcing material can be demulsified under a light-triggered condition, effective components of the reinforcing material can block concrete gaps, and the surface performance of concrete is remarkably improved; and the photosensitive material can form a durable coating on the surface of the concrete, so that the concrete has a self-cleaning function.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a self-cleaning concrete surface strengthening material and a preparation method thereof. Background Art

[0002] With the continuous development of modern high-performance concrete technology and the increasing innovation of building materials and structural design technology, high-end concrete has been widely used in various fields, but the problems it faces are also increasing. Such as surface weathering, sulfate corrosion, acid corrosion, alkali corrosion and mechanical wear, especially concrete carbonization and chloride ion erosion, which will cause steel corrosion and further accelerate the deterioration of concrete. These problems not only reduce the service life of concrete, but also increase maintenance and repair costs.

[0003] Concrete surface strengthening materials can improve the surface properties of concrete, such as compression, tension, wear, frost and chemical corrosion resistance, through penetration crystallization, pore blocking and surface film formation. At present, there are many types of concrete surface strengthening materials on the market, but there are still some problems in their research and application, such as insufficient penetration, low strength of crystallized products, single function, long-term, durability and environmental friendliness still need further verification. With the increasing demand for high-end construction and landscape engineering, it is of great significance to develop concrete surface strengthening materials with simple preparation process, strong penetration and multifunctionality.

[0004] Patent CN113105264 B discloses a surface enhancer for long-term concrete and its preparation method. The surface enhancer is a microcapsule composed of an inner core layer, an outer shell and a calcium supplement component. First, a nano-SiO2 solution is slowly poured into a highly water-absorbent nano-microsphere aqueous solution under rapid stirring to obtain a highly water-absorbent nano-microsphere / SiO2 composite solution; then, a Ca-containing nano-microsphere / SiO2 composite solution is successively added to the capsule wall material A. 2+ The Ca content of solution and capsule wall material B 2+ Solution, forming a microcapsule consisting of an inner core layer, an outer shell, and a calcium supplement component. This method has many steps and a long process, and is not suitable for large-scale production; the stress required for the capsule to rupture is large, and the scope of application is limited.

[0005] Patent CN113754468 A discloses a concrete surface enhancer, including 80-90 parts of the main reinforcing raw material; 5-8 parts of negative ion powder; 1-3 parts of nano titanium dioxide; 1-3 parts of rare earth oxide; 4-5 parts of graphene powder; 0.5-0.8 parts of stabilizer, wherein the negative ion particles are 2-5 parts of Bian stone, 1-2 parts of tourmaline, 2-3 parts of strange ice stone, and 1-2 parts of magnet. The enhancer improves the surface performance of concrete and enables the concrete to release negative ions uniformly, improves the quality of the surrounding environment, has a health-care effect on the human body, and has multifunctionality, but the specific release amount and the health-care effect on the human body need further verification.

[0006] Patent CN 114014984 A discloses a microgel concrete surface enhancer and its preparation method, the enhancer includes 920-970 parts of core-shell microgel, 0.5-4 parts of titanium salt, 2-18 parts of organic titanium, 0.8-4 parts of organic chromium, 0.1-1 parts of manganese salt, 0.2-2 parts of organic manganese and 0.1-1.5 parts of organic magnesium. The microgel with core-shell structure is loaded with enhanced organic metals and compounds, which has the characteristics of high strength, high temperature resistance, aging resistance, acid and alkali resistance, etc., but the microgel loaded with active ingredients may hinder their release, resulting in insufficient penetration depth.

[0007] In general, the current development of concrete surface strengthening materials mainly has the following three problems: ① The process of preparing concrete surface strengthening materials is complicated and not suitable for large-scale production; ② The specially designed structure leads to limited release of internal effective reinforcing components, which in turn leads to insufficient penetration depth and insufficient surface strengthening; ③ The function is single, and the long-term, durability and environmental friendliness are insufficient, which cannot meet the needs of high-end construction and landscape engineering fields. Summary of the invention

[0008] 1. Technical problems to be solved:

[0009] In view of the above technical problems, the present invention provides a self-cleaning concrete surface strengthening material and a preparation method thereof. The strengthening material is a microspherical configuration emulsion with a water-in-oil-in-water (W1 / O / W2) three-layer structure, wherein the internal water phase is composed of fluorosilicates, nano-oxides, silicates, sulfates and co-solvents, etc., and the components are effective ingredients that need to be protected and controlled for release; the middle oil phase is a trifluoromethylphenylsilanepyrazole azo compound, which serves as a photosensitive reaction layer to wrap the internal components; the outermost water phase is composed of a permeation promoter and a dispersant, which covers the internal emulsion and protects the emulsion from damage in a non-light-triggered environment.

[0010] 2. Technical solution:

[0011] A self-cleaning concrete surface strengthening material, characterized by: a microspherical configuration emulsion with a three-layer structure of water-in-oil-in-water; an inner water phase of which is a mixed solution composed of fluorosilicate, nano-oxide, silicate, sulfate and co-solvent; an oil phase of which is a trifluoromethylphenylsilane pyrazole azo compound; and an outer water phase composed of a penetration promoter and a dispersant.

[0012] A method for preparing a self-cleaning concrete surface strengthening material comprises the following steps:

[0013] Step 1: Mix fluorosilicate, nano oxide, silicate, sulfate, co-solvent and water in a preset ratio to form a uniform solution W1; mix a penetration enhancer, a dispersant and water in a preset ratio to form a uniform solution W2;

[0014] Step 2: slowly add emulsifier 1 and trifluoromethylphenylsilane pyrazole azo compound to the uniform solution W1 in sequence, and emulsify the mixed solution by a high-pressure homogenizer under a preset working pressure to obtain a white uniform primary W1 / O emulsion;

[0015] Step 3: Mix emulsifier 2 and solution W2 evenly to obtain solution A; pass solution A and the primary W1 / O emulsion into a microfluidic emulsification device, and achieve secondary emulsification of the primary W1 / O emulsion by adjusting the flow rate ratio of the two to obtain a white, uniform three-layer microspherical W1 / O / W2 emulsion, that is, a self-cleaning concrete surface strengthening material.

[0016] Furthermore, the uniform solution W1 is prepared in the following proportions: by weight, 4-6 parts of fluorosilicate, 4-8 parts of nano oxide, 7-10 parts of silicate, 0.5-1.5 parts of sulfate, 0.1-0.8 parts of co-solvent, and water is added to make up to 100 parts.

[0017] Furthermore, the uniform solution W2 is prepared in the following proportions: by weight, 0.1-0.3 parts of a permeation enhancer, 0.5-0.8 parts of a dispersant, and water to make up to 100 parts.

[0018] Furthermore, the trifluoromethylphenylsilane pyrazole azo compound is a photosensitive substance. The compound can change its molecular form under light conditions, from the dominant E state to the metastable Z state. Its structure is shown as follows:

[0019]

[0020] In the above formula, n is an integer of 1 to 11; R is one of -OCH3, -OCH2CH3, -OCH2CH2CH3, -OC6H5, and -OCH=CH2.

[0021] Furthermore, the fluorosilicate is one or more combinations of sodium fluorosilicate, magnesium fluorosilicate, potassium fluorosilicate, ammonium fluorosilicate, and lithium fluorosilicate; the nano oxide is one or more combinations of nano SiO2, nano TiO2, nano Al2O3, and nano ZnO; the silicate is one or more combinations of sodium silicate, potassium silicate, and lithium silicate; the sulfate is one or more combinations of sodium sulfate, potassium sulfate, lithium sulfate, and magnesium sulfate; the co-solvent is one or more combinations of polyethylene glycol, polyvinyl pyrrolidone, sodium polyacrylate, and polyvinyl alcohol.

[0022] Furthermore, the penetration enhancer is one or a combination of lauric acid and polysorbate 80; the dispersant is one or a combination of sodium lauryl sulfate, capric glycine, and dodecyl glucoside.

[0023] Furthermore, the emulsifier 1 is one or more of Span 80, cetyl alcohol, polydimethylsiloxane, and cyclomethicone; and the emulsifier 2 is one or more of fluorocarbon alcohol ethoxylate, sodium perfluoroalkyl sulfonate, sodium perfluorocarboxylate, and perfluoroalkylamine.

[0024] Furthermore, the preset working pressure of the high-pressure homogenizer is 10-50 MPa and the power is 2 kW.

[0025] Furthermore, the flow rate ratio of solution A and primary W1 / O emulsion introduced into the microfluidic emulsification device is 5:1-10:1; wherein the flow rate of solution A is 10-100 μL / min.

[0026] 3. Beneficial effects:

[0027] (1) The self-cleaning concrete surface strengthening material prepared by the present invention has a microspherical configuration emulsion with a three-layer structure of water-in-oil-in-water (W1 / O / W2). The emulsion with this special structure wraps the effective ingredients of the strengthening material inside, which can protect them and control their release.

[0028] (2) The structure of the self-cleaning concrete surface strengthening material prepared by the present invention is a microspherical configuration emulsion with a three-layer structure of water-in-oil-in-water (W1 / O / W2), and the middle oil phase layer is a special trifluoromethylphenylsilane pyrazole azo compound, which is a photosensitive substance. Its morphology changes under light conditions, causing stress changes between the emulsion layers, thereby achieving light-triggered demulsification and simplifying construction operations. The azo compound in the balanced middle oil phase layer under light-proof conditions establishes a dominant E state with a lower intensity. After the reinforcing material is evenly applied to the concrete surface, it is switched to light conditions, driving the azo compound in the middle oil phase layer into a metastable Z state, and its structure changes. This transformation will cause stress changes between the emulsion (W1 / O / W2) layers, destroying the emulsion stability and causing demulsification.

[0029] (3) The self-cleaning concrete surface strengthening material prepared by the present invention, after demulsification, the silanol groups of the aromatic pyrazole azo compound in the middle layer can form a stable silicon oxygen (Si-O-Si) bond with the concrete surface, forming a strong and durable coating on the concrete surface. Under sunlight or dark conditions, the azo compound morphology changes, the -CF3 bond or -N=N- bond is exposed, giving the concrete surface interactive hydrophobic or oleophobic properties, realizing the self-cleaning function.

[0030] (4) The self-cleaning concrete surface strengthening material prepared by the present invention has its internal strengthening components flow out at the same time after demulsification, and penetrate into the interior of the concrete along the capillary pores of the concrete under the action of a penetration promoter, etc., and seal the capillary pores of the concrete while reacting with substances such as Ca(OH)2 inside the concrete to form a high-strength crystalline product, thereby greatly improving the surface performance of the concrete.

[0031] In summary, the self-cleaning concrete surface strengthening material prepared by the present invention has a simple preparation process, easy operation, and can prevent sagging during construction; the effective ingredients have a deep penetration depth, the crystallized product has high strength, can block the pores of the concrete, and significantly improve the surface performance of the concrete, meeting the needs of different fields such as high-end construction and landscape engineering. DETAILED DESCRIPTION

[0032] The embodiments of the present invention are described in detail, implemented under the premise of the technical solution of the present invention, and detailed implementation methods and operating processes are given, but the protection scope of the present invention is not limited to the following embodiments. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight.

[0033] Embodiment 1:

[0034] Step S01: 4 parts of sodium fluorosilicate, 4 parts of nano-SiO2, 7 parts of potassium silicate, 0.5 parts of lithium sulfate, 0.1 parts of polyethylene glycol and 84.4 parts of water are mixed evenly to form a uniform solution W1; 0.1 parts of lauric acid, 0.5 parts of sodium dodecyl sulfate and 99.4 parts of water are mixed evenly to form a uniform solution W2. Step S02: Span80 and trifluoromethylphenylsilane pyrazole azo compound (structural formula shown below) are slowly added to the uniform solution W1 in sequence, and the mixed solution is emulsified by a high-pressure homogenizer at 10MPa to obtain a white uniform primary W1 / O emulsion. Step S03: The fluorocarbon alcohol ethoxylate and the uniform solution W2 are mixed evenly to obtain solution A. The microfluidic emulsification technology is used, and the flow rate ratio of solution A to the primary W1 / O emulsion is 5:1. When the flow rate of solution A is 10 μL / min, it is emulsified with the primary W1 / O emulsion for a second time to obtain a white uniform three-layer microspherical configuration emulsion (W1 / O / W2), that is, a self-cleaning concrete surface strengthening material.

[0035]

[0036] Embodiment 2:

[0037] Step S01: 6 parts of magnesium fluorosilicate, 8 parts of nano-TiO2, 10 parts of sodium silicate, 1.5 parts of potassium sulfate, 0.8 parts of polyvinyl pyrrolidone and 73.7 parts of water are mixed evenly to form a uniform solution W1; 0.3 parts of polysorbate-80, 0.8 parts of glycine decanoate and 98.9 parts of water are mixed evenly to form a uniform solution W2. Step S02: Cetyl alcohol and trifluoromethylphenylsilane pyrazole azo compound (structural formula shown below) are slowly added to the uniform solution W1 in sequence, and the mixed solution is emulsified by a high-pressure homogenizer at 50MPa to obtain a white uniform primary W1 / O emulsion. Step S03: Sodium perfluoroalkyl sulfonate and uniform solution W2 are mixed evenly to obtain solution A. The flow rate ratio of solution A and the primary W1 / O emulsion is controlled to be 10:1 by microfluidic emulsification technology. When the flow rate of solution A is 100 μL / min, it is emulsified with the primary W1 / O emulsion for a second time to obtain a white uniform three-layer microspherical configuration emulsion (W1 / O / W2), that is, a self-cleaning concrete surface strengthening material.

[0038]

[0039] Embodiment 3:

[0040] Step S01: 5 parts of magnesium fluorosilicate, 6 parts of nano ZnO, 8 parts of lithium silicate, 1 part of sodium sulfate, 0.4 parts of sodium polyacrylate and 79.6 parts of water are mixed evenly to form a uniform solution W1; 0.2 parts of lauric acid, 0.6 parts of dodecyl glucoside and 99.2 parts of water are mixed evenly to form a uniform solution W2. Step S02: Polydimethylsiloxane and trifluoromethylphenylsilane pyrazole azo compound (structural formula shown below) are slowly added to the uniform solution W1 in sequence, and the mixed solution is emulsified by a high-pressure homogenizer at 30MPa to obtain a white uniform primary W1 / O emulsion. Step S03: Sodium perfluorocarboxylate and uniform solution W2 are mixed evenly to obtain solution A. The flow rate ratio of solution A and primary W1 / O emulsion is controlled to be 8:1 by microfluidic emulsification technology. When the flow rate of solution A is 70 μL / min, it is emulsified with the primary W1 / O emulsion for a second time to obtain a white uniform three-layer microspherical configuration emulsion (W1 / O / W2), i.e., a self-cleaning concrete surface strengthening material.

[0041]

[0042] Embodiment 4:

[0043] Step S01: 5 parts of sodium fluorosilicate, 5 parts of nano-SiO2, 7 parts of lithium silicate, 0.8 parts of potassium sulfate, 0.3 parts of polyvinyl alcohol and 81.9 parts of water are mixed evenly to form a uniform solution W1; 0.2 parts of polysorbate-80, 0.6 parts of sodium dodecyl sulfate and 99.2 parts of water are mixed evenly to form a uniform solution W2. Step S02: Cyclomethylsiloxane and trifluoromethylphenylsilane pyrazole azo compound (structural formula shown below) are slowly added to the uniform solution W1 in sequence, and the mixed solution is emulsified by a high-pressure homogenizer at 20MPa to obtain a white uniform primary W1 / O emulsion. Step S03: The perfluoroalkylamine and the uniform solution W2 are mixed evenly to obtain solution A. The flow rate ratio of solution A and the primary W1 / O emulsion is controlled to be 6:1 by microfluidic emulsification technology. When the flow rate of solution A is 30 μL / min, it is emulsified with the primary W1 / O emulsion for a second time to obtain a white uniform three-layer microspherical configuration emulsion (W1 / O / W2), that is, a self-cleaning concrete surface strengthening material.

[0044]

[0045] Embodiment 5:

[0046] Step S01: 6 parts of sodium fluorosilicate, 7 parts of nano-SiO2, 9 parts of potassium silicate, 0.8 parts of magnesium sulfate, 0.6 parts of polyethylene glycol and 76.6 parts of water are mixed evenly to form a uniform solution W1; 0.2 parts of lauric acid, 0.6 parts of capric glycine and 99.2 parts of water are mixed evenly to form a uniform solution W2. Step S02: Span80 and trifluoromethylphenylsilane pyrazole azo compound (structural formula shown below) are slowly added to the uniform solution W1 in sequence, and the mixed solution is emulsified by a high-pressure homogenizer at 40MPa to obtain a white uniform primary W1 / O emulsion. Step S03: The fluorocarbon alcohol ethoxylate and the uniform solution W2 are mixed evenly to obtain solution A. The microfluidic emulsification technology is used to control the flow rate ratio of solution A and the primary W1 / O emulsion to be 7:1. At a flow rate of 60 μL / min, solution A is emulsified with the primary W1 / O emulsion for a second time to obtain a white, uniform three-layer microspherical configuration emulsion (W1 / O / W2), which is a self-cleaning concrete surface strengthening material.

[0047]

[0048] Test example: Rebound strength, long-term performance and durability of concrete

[0049] Several C30 concrete specimens were formed. After curing for 28 days, the samples obtained in Examples 1 to 5 and two commercially available concrete surface enhancers were coated on the surface of the specimens. The rebound strength before applying the concrete surface enhancer and 7 days and 28 days after applying the concrete surface enhancer was tested with reference to JGJ / 123-2001 "Technical Specification for Testing Concrete Compressive Strength by Rebound Method"; the durability of concrete was tested with reference to GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete".

[0050] Table 1. Changes in concrete properties after painting different samples

[0051]

[0052]

[0053] As can be seen from Table 1, after the self-cleaning concrete surface strengthening material prepared by the present invention is applied, the rebound strength of the concrete is significantly improved. The 7d rebound strength can generally be increased by about 10MPa, and the 28d rebound strength can generally be increased by about 11MPa, which is slightly better than similar products on the market. At the same time, the durability of the concrete after application is also significantly improved.

[0054] Test example: Concrete surface self-cleaning performance

[0055] The samples obtained in Examples 1 to 5 and two commercially available hydrophobic and oleophobic coatings were coated on the concrete surface, and the hydrophobic and oleophobic properties of the concrete surface were tested using a contact angle meter. The results are shown in Table 2.

[0056] Table 2 Contact angles of different solutions on the surface of concrete specimens

[0057]

[0058] As can be seen from Table 2, when the self-cleaning concrete surface strengthening material prepared by the present invention is applied to the concrete surface, the concrete can exhibit interactive hydrophobic or oleophobic properties under illumination or non-illumination conditions, realize the self-cleaning function, and meet the needs of high-end concrete.

[0059] Although the present invention has been disclosed as above in terms of preferred embodiments, they are not intended to limit the present invention. Anyone skilled in the art can make various changes or modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection defined by the claims of this application.

Claims

1. A self-cleaning concrete surface strengthening material, Features: It is a microspherical emulsion with a three-layer structure of water-in-oil-in-water; its inner water phase is a mixed solution of fluorosilicate, nano-oxide, silicate, sulfate and co-solvent; the oil phase is trifluoromethylphenylsilane pyrazole azo compound; and the outer water phase is composed of a penetration enhancer and a dispersant.

2. A method for preparing a self-cleaning concrete surface strengthening material, for preparing the self-cleaning concrete surface strengthening material as claimed in claim 1, Features: The following steps are involved: Step 1: Evenly mix fluorosilicate, nano oxide, silicate, sulfate, co-solvent and water according to a preset ratio to prepare a uniform solution W1; The penetration enhancer, dispersant and water are mixed evenly according to a preset ratio to prepare a uniform solution W2; Step 2: slowly add emulsifier 1 and trifluoromethylphenylsilane pyrazole azo compound to the uniform solution W1 in sequence, and emulsify the mixed solution by a high-pressure homogenizer under a preset working pressure to obtain a white uniform primary W1 / O emulsion; Step 3: Mix emulsifier 2 and solution W2 evenly to obtain solution A; pass solution A and the primary W1 / O emulsion into a microfluidic emulsification device, and achieve secondary emulsification of the primary W1 / O emulsion by adjusting the flow rate ratio of the two to obtain a white, uniform three-layer microspherical W1 / O / W2 emulsion, that is, a self-cleaning concrete surface strengthening material.

3. The method for preparing a self-cleaning concrete surface strengthening material according to claim 2, Features: The proportions for preparing the uniform solution W1 are as follows: by weight, 4-6 parts of fluorosilicate, 4-8 parts of nano oxide, 7-10 parts of silicate, 0.5-1.5 parts of sulfate, 0.1-0.8 parts of co-solvent, and water to make up to 100 parts.

4. The method for preparing a self-cleaning concrete surface strengthening material according to claim 2, Features: The proportions for preparing the uniform solution W2 are as follows: by weight, 0.1-0.3 parts of the penetration enhancer, 0.5-0.8 parts of the dispersant, and water to make up to 100 parts.

5. The method for preparing a self-cleaning concrete surface strengthening material according to claim 2, Features: Trifluoromethylphenylsilane pyrazole azo compound is a photosensitive substance. The compound can change its molecular form under light conditions, from the dominant E state to the metastable Z state. Its structure is shown as follows: In the above formula, n is an integer from 1 to 11; R is -OCH 3 、-OCH 2 CH 3 、-OCH 2 CH 2 CH 3 、-OC 6 H 5 、-OCH=CH 2 One of them.

6. The method for preparing a self-cleaning concrete surface strengthening material according to claim 2, Features: The fluorosilicate is one or a combination of sodium fluorosilicate, magnesium fluorosilicate, potassium fluorosilicate, ammonium fluorosilicate, and lithium fluorosilicate; the nano oxide is nano SiO 2 、Nano-TiO 2 、Nano Al 2 O 3 , nano ZnO; the silicate is one or more combinations of sodium silicate, potassium silicate, and lithium silicate; the sulfate is one or more combinations of sodium sulfate, potassium sulfate, lithium sulfate, and magnesium sulfate; the co-solvent is one or more combinations of polyethylene glycol, polyvinyl pyrrolidone, sodium polyacrylate, and polyvinyl alcohol.

7. The method for preparing a self-cleaning concrete surface strengthening material according to claim 2, Features: The penetration enhancer is one or a combination of lauric acid and polysorbate-80; the dispersant is one or a combination of sodium lauryl sulfate, capric glycine, and dodecyl glucoside.

8. The method for preparing a self-cleaning concrete surface strengthening material according to claim 2, Features: The emulsifier 1 is one or more of Span 80, cetyl alcohol, polydimethylsiloxane, and cyclomethicone; the emulsifier 2 is one or more of fluorocarbon alcohol ethoxylate, sodium perfluoroalkyl sulfonate, sodium perfluorocarboxylate, and perfluoroalkylamine.

9. The method for preparing a self-cleaning concrete surface strengthening material according to claim 2, Features: The preset working pressure of the high-pressure homogenizer is 10-50 MPa and the power is 2 kW.

10. The method for preparing a self-cleaning concrete surface strengthening material according to claim 2, Features: The flow rate ratio of solution A and primary W1 / O emulsion passed into the microfluidic emulsification device is 5:1-10:1; wherein the flow rate of solution A is 10-100 μL / min.

Citation Information

Cited By

  • Concrete shrinkage inhibition and compensation spray liquid

    TWI940393B