Carbomer resin and preparation method thereof
The staged addition of α,β-unsaturated acid alcohol ester monomers during carbomer resin polymerization addresses compatibility issues, resulting in alcohol gels with improved viscosity and transparency.
Patent Information
- Application Number
- CN202410957879.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-12-03
AI Technical Summary
Carbomer resins exhibit poor compatibility with alcohol substances, leading to slow swelling in alcohol solutions, resulting in gels with poor transparency, turbidity, and viscosity issues.
A method involving staged addition of α,β-unsaturated acid alcohol ester monomers during polymerization with α,β-unsaturated acid and α,β-unsaturated acid alkyl ester monomers, optimizing viscosity values to enhance compatibility and uniformity, allowing for rapid swelling and improved viscosity and transparency in alcohol gels.
The prepared carbomer resin demonstrates excellent compatibility with alcohol substances, enabling rapid swelling and producing gels with enhanced viscosity and light transmittance, suitable for high-end applications.
Smart Images

Figure CN119060236A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new material preparation and thickener, and in particular to a carbomer resin and a preparation method thereof. Background Art
[0002] Carbomer resin is a kind of high molecular polymer with a certain cross-linked structure. Its main component is cross-linked polyacrylic acid or cross-linked polyacrylic acid (ester) macromolecules. Its homopolymer and copolymer swell in water and can form gel after adding an appropriate amount of alkaline neutralizer, thereby providing excellent stability and thickening performance for the surfactant system. In addition, carbomer resin also has the advantages of high stability and good transparency, so it is widely used in many fields such as daily chemicals, medicine and health, and personal care products.
[0003] With the growth of market demand for high-end applications, carbomer resins are increasingly being used in the preparation of polar solvent gels such as alcohol and water. However, when traditional carbomer resins come into contact with alcohol solutions, a dense "water layer" protective film will form on the resin surface, making it difficult for the resin to swell in alcohol solvents. The viscosity and transmittance of the alcohol gel obtained after subsequent alkali neutralization are not ideal, and cannot meet the application requirements of high-end products. In addition, traditional carbomer resins have a multi-carboxyl structure on the surface and have poor compatibility with alcohol substances, which will result in unsatisfactory viscosity of the prepared alcohol gel.
[0004] In order to solve the above problems, unsaturated alkyl ester hydrophobic monomers are often introduced in the existing carbomer resin synthesis process. By modifying some hydrophobic groups on the surface of the macromolecule, it is difficult to form a dense "water layer" during the swelling process in the alcohol solution, thereby promoting the rapid swelling of the carbomer resin in the alcohol solution. However, this method cannot solve the problem of poor compatibility between the carbomer resin macromolecule and alcohol substances. There are both hydrophilic and hydrophobic segments in the macromolecular structure of the prepared carbomer resin. During the swelling process of the alcohol solution, some water molecules cannot fully diffuse and fill the internal gaps of the macromolecular chain. Therefore, the macromolecular segments cannot be fully stretched in the solvent. After subsequent alkali neutralization, some frozen segments are prone to a decrease in local refractive index, which will eventually lead to poor apparent transparency and turbidity of the prepared alcohol gel, and poor viscosity performance. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention discloses a carbomer resin and a preparation method thereof. The preparation method of the carbomer resin aims to solve the problem that the carbomer resin has poor compatibility with alcohol substances and cannot swell quickly in alcohol substances, thereby causing the prepared gel to have poor transparency, turbidity, and poor viscosity performance.
[0006] In order to achieve the above technical objectives, on the one hand, the present invention provides a method for preparing a carbomer resin, the method comprising: in an inert atmosphere, an α,β-unsaturated acid monomer, an α,β-unsaturated acid alkyl ester monomer, a surfactant, a crosslinking agent and a first initiator are subjected to a polymerization reaction in an organic solvent; when the viscosity of the reaction system reaches a first viscosity value, the α,β-unsaturated acid alcohol ester monomer is added to the reaction system for the first time to continue the polymerization reaction; when the viscosity of the reaction system reaches a second viscosity value, a second initiator is added to the reaction system and the α,β-unsaturated acid alcohol ester monomer is added for the second time; after the polymerization reaction is completed, the carbomer resin is obtained; wherein the second viscosity value is greater than the first viscosity value.
[0007] The research and development team of the present invention added α, β-unsaturated acid alcohol ester monomers to carry out copolymerization reaction during the preparation of carbomer resin using α, β-unsaturated acid monomers and α, β-unsaturated acid alkyl ester monomers as raw materials, thereby improving the compatibility of the macromolecular segments of the prepared carbomer resin with alcohol substances, allowing the solvent molecules to freely diffuse into the gaps in the macromolecular segments during the dispersion of the alcohol substances, so that the macromolecular chains can be fully stretched, and the viscosity and light transmittance of the prepared gel can be significantly improved after subsequent neutralization.
[0008] In addition, the research and development team adopted a phased addition method in the above technical scheme, adding α, β-unsaturated acid alcohol ester monomers to the reaction system twice: specifically, based on a large amount of experimental data, the research and development team added the α, β-unsaturated acid alcohol ester monomers for the first time when the viscosity of the reaction system reached a first viscosity value, which can avoid the uneven distribution of monomers in the polymer due to differences in the reactivity rates of each monomer, thereby improving the uniformity of the distribution of the α, β-unsaturated acid polyol ester monomers in the polymer; further, when the viscosity of the reaction system reaches a second viscosity value, the α, β-unsaturated acid alcohol ester monomer and the second initiator are added again to continue the polymerization reaction, so that the monomer polymerization can be initiated again on the macromolecular chain that has been polymerized to form a side chain rich in α, β-unsaturated acid polyol ester monomers, thereby improving the compatibility of the carbomer resin with alcohol substances and accelerating the swelling of the prepared carbomer resin in the alcohol solution.
[0009] It should be noted that the technical solution of the present invention is not limited to the method for detecting the viscosity value of the staged reaction system. Those skilled in the art may choose to use an online viscometer, or other equipment or operation method to monitor the viscosity of the reaction system in real time, and the technical solutions formed thereby are all within the protection scope of the present invention.
[0010] It should be noted that the present invention does not limit the specific operation of adding the α,β-unsaturated acid monomer, α,β-unsaturated acid alkyl ester monomer, surfactant, cross-linking agent and first initiator to the organic solvent. Those skilled in the art may choose to add each component to the organic solvent separately and mix them evenly, and then heat them to a certain temperature for polymerization reaction, or may choose to first mix the α,β-unsaturated acid monomer, α,β-unsaturated acid alkyl ester monomer, surfactant and cross-linking agent in the organic solvent evenly, heat them to a certain temperature and then add the first initiator for polymerization reaction, or may choose to adopt other adding methods, and the technical solutions formed thereby are all within the protection scope of the present invention.
[0011] It should be noted that the present invention does not limit the specific operation method of adding the α, β-unsaturated acid alcohol ester monomer to the reaction system. The dripping method can be selected to control the reaction rate. Those skilled in the art can select other methods of adding the α, β-unsaturated acid alcohol ester monomer through non-creative labor, and the technical solutions formed thereby are all within the protection scope of the present invention.
[0012] In a further example of the present invention, the timing of adding α,β-unsaturated acid alcohol ester monomers to the reaction system in stages is explored and optimized. Based on a large amount of experimental data, the research and development team of the present invention can select the first viscosity value as 1000-5000cP, preferably 2000-4000cP, and further preferably 2000-3500cP. The embodiments of the present invention show the viscosity and light transmittance of alcohol gel prepared by carbomer resin prepared at different first viscosity values.
[0013] In a further example of the present invention, the second viscosity value is the peak viscosity value of the reaction system after the first addition of the α,β-unsaturated acid alcohol ester monomer. It should be noted that the peak viscosity value of the reaction system after the first addition of the α,β-unsaturated acid alcohol ester monomer in the present invention refers to the viscosity when the viscosity of the reaction system continues to increase until it no longer increases; in the embodiment of the present invention, the research and development team found through viscosity monitoring that the second viscosity value can be selected from about 3000-10000cP, further selected from about 6000-9000cP, and further selected from about 7000-8500cP.
[0014] In a further example of the present invention, the type of the α,β-unsaturated alcohol ester monomer and the amount of the phased addition are explored and optimized. Optionally, the α,β-unsaturated acid alcohol ester monomer includes one or more of polyethylene glycol (200) acrylate, polyethylene glycol (600) acrylate, polyethylene glycol (1000) acrylate, poly 1,3-propylene glycol (200) acrylate, octanediol acrylate, 12-hydroxylauryl alcohol acrylate, and 12-hydroxystearyl alcohol acrylate; optionally, the mass of the α,β-unsaturated acid alcohol ester monomer added for the first time is 0.5%-10% of the mass of the α,β-unsaturated acid monomer; preferably 2%-8%; optionally, the mass of the α,β-unsaturated acid alcohol ester monomer added for the second time is 0.1%-2% of the mass of the α,β-unsaturated acid monomer; preferably 0.5%-2%; it is also worth noting that the present invention does not limit the types of the α,β-unsaturated acid alcohol ester monomers added for the first and second times, and the types of the α,β-unsaturated acid alcohol ester monomers added for the first time and the α,β-unsaturated acid alcohol ester monomers added for the second time are the same or different.
[0015] In a further example of the present invention, the type and amount of the α,β-unsaturated acid monomer are explored and optimized. Optionally, the α,β-unsaturated acid monomer includes one or more of acrylic acid, methacrylic acid, maleic acid, crotonic acid and itaconic acid; Optionally, the mass of the α,β-unsaturated acid monomer is 5%-20% of the mass of the organic solvent.
[0016] In a further example of the present invention, the type and amount of the α,β-unsaturated acid alkyl ester monomer are explored and optimized. Optionally, the α,β-unsaturated acid alkyl ester monomer includes one or more of methyl acrylate, isooctyl acrylate, stearic acrylate, lauryl acrylate and palmitic acrylate; Optionally, the mass of the α,β-unsaturated acid alkyl ester monomer is 0.5%-10% of the mass of the α,β-unsaturated acid monomer.
[0017] In a further example of the present invention, the type and amount of the surfactant are optimized. The surfactant includes an organic surfactant and an inorganic surfactant. When the surfactant is an inorganic surfactant, it can optionally include one or more of potassium carbonate, sodium carbonate, sodium chloride, potassium chloride, calcium chloride and sodium bicarbonate; when the surfactant is an organic surfactant, it can optionally include one or more of Tween-20, Tween-80, Span-60, Span-80, Oleth-10 and hydroxyethyl cellulose. Optionally, the mass of the inorganic surfactant is 0.1%-5% of the mass of the α,β-unsaturated acid monomer. Optionally, the mass of the organic surfactant is 0.1%-5% of the mass of the α,β-unsaturated acid monomer.
[0018] In a further example of the present invention, the type and amount of the cross-linking agent are explored and optimized. Optionally, the cross-linking agent is a cross-linking agent containing at least two unsaturated carbon-carbon double bonds; Optionally, the cross-linking agent includes one or more of pentaerythritol diallyl ether, pentaerythritol triallyl ether, pentaerythritol triacrylate, diallyl phthalate, ethylene glycol dimethacrylate and allyl sucrose ether; Optionally, the mass of the cross-linking agent is 0.1%-5% of the mass of the α,β-unsaturated acid monomer.
[0019] In a further example of the present invention, the composition of the organic solvent is explored and optimized. Optionally, the organic solvent is composed of a polar organic solvent and a non-polar organic solvent; further optionally, the polar organic solvent includes one or more of acetonitrile, acetic acid, ethyl acetate, butyl acetate, toluene and tetrahydrofuran; further optionally, the non-polar organic solvent includes one or more of benzene, cyclohexane, carbon tetrachloride and dichloromethane; optionally, the mass of the polar organic solvent is 20%-80% of the mass of the organic solvent.
[0020] In a further example of the present invention, the polymerization reaction temperature may be selected to be 50-90° C. to increase the reaction rate and polymerization efficiency.
[0021] It should be noted that the preparation process of the present invention can be carried out under stirring conditions, and the stirring rate can be selected to be 200-400 rpm; in a further example of the present invention, after adding a second initiator and a second addition of the α,β-unsaturated acid alcohol ester monomer to the reaction system, the reaction is stirred for 1-3 hours to obtain the carbomer resin.
[0022] In a further example of the present invention, the types and amounts of the first initiator and the second initiator are explored and optimized. Optionally, the first initiator and the second initiator are independently selected from one or more of dodecyl peroxide, benzoyl peroxide, azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptylonitrile and dimethyl azobisisobutyrate. In the actual preparation process, the types of the first initiator and the second initiator can be selected to be the same or different. Optionally, the mass of the first initiator is 0.1%-5% of the mass of the α,β-unsaturated acid monomer. Optionally, the mass of the second initiator is 0.1%-5% of the mass of the α,β-unsaturated acid alcohol ester monomer added for the second time, further 0.5%-4%, and further 0.5%-2.5%.
[0023] In a further example of the present invention, the present invention also includes a process of post-treating the prepared carbomer resin after completing the polymerization reaction. Specifically, the obtained carbomer resin can be washed, filtered and dried to remove impurities, improve product purity and stability, and facilitate the storage and transportation of the product. The present invention does not limit the specific post-treatment operation, and those skilled in the art can perform post-treatment of the carbomer resin based on the present invention through non-creative labor, and the technical solutions formed thereby are all within the scope of protection of the present invention.
[0024] It should be noted that in the present invention, the inert atmosphere refers to a gas environment composed of gases that do not chemically interact with the reactants, such as a nitrogen atmosphere, or an atmosphere formed by a gas of the zeroth group element in the periodic table (such as argon).
[0025] It should be noted that the present invention does not limit the reaction equipment for the polymerization reaction. Those skilled in the art can select equipment and facilities suitable for the preparation of carbomer resin according to actual working conditions, and the technical solutions thus formed are all within the protection scope of the present invention.
[0026] On the other hand, the present invention provides a carbomer resin prepared by the above-mentioned carbomer resin preparation method.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] In the process of preparing carbomer using α,β-unsaturated acid monomers and α,β-unsaturated acid alkyl ester monomers as raw materials, α,β-unsaturated acid alcohol ester monomers are added in two stages based on the viscosity value of the reaction system for copolymerization reaction, the prepared carbomer resin has excellent compatibility with alcohol substances, can be rapidly swollen in alcohol substances, and the prepared gel has excellent viscosity and light transmittance. The preparation method of the present invention is simple to operate and easy to be produced on an industrial scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0030] Figure 1 A comparison chart of the light transmittance of the gel obtained after the carbomer resin prepared in Example 7 and Comparative Example 2 was swollen with alcohol is shown. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are given. However, it should be understood that these embodiments are only used for more detailed description and should not be understood as limiting the present invention in any form, i.e., not intended to limit the scope of protection of the present invention.
[0032] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.
[0033] It should be noted that, in the description of the preferred embodiment, unless otherwise clearly specified and limited, the terms "first time" and "second time" are used for descriptive purposes only. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances, and therefore they cannot be understood as limitations on the present invention.
[0034] It should be noted that in the embodiments and comparative examples of the present invention, the transmittance and viscosity of the prepared carbomer resin after swelling in alcohol are measured to characterize the performance of the carbomer resin in alcoholic substances, but this does not limit the scope of protection of the present invention; specifically, the alcohol gel transmittance and viscosity test adopts the following method:
[0035] Alcohol gel transmittance test: accurately weigh 497.5g of 75% alcohol into a 1000mL beaker, place it in a 25℃ constant temperature box, and in a static state, quickly and evenly sprinkle 2.5g of carbomer resin product on the water surface, and stir for 4 hours after the polymer product is completely settled; then, add triethanolamine to the solution under stirring to neutralize the polymer, and adjust the pH of the resulting alcohol gel to 7.0-7.8; then transfer the alcohol gel to a centrifuge tube and centrifuge it at 5000rpm for 30min for defoaming treatment; use Shimadzu UV-1800 ultraviolet spectrophotometer to measure the transmittance of the gel at 420nm at 25℃.
[0036] Alcohol gel viscosity test: accurately weigh 497.5g of 75% alcohol into a 1000mL beaker, place it in a 25℃ constant temperature box, and in a static state, quickly and evenly sprinkle 2.5g of carbomer resin product on the water surface, and stir for 4 hours after the polymer product is completely settled; then, add triethanolamine to the solution under stirring to neutralize the polymer, and adjust the pH of the resulting alcohol gel to 7.0-7.8; then transfer the alcohol gel to a centrifuge tube and centrifuge it at 5000rpm for 30min for defoaming treatment; measure the viscosity of the alcohol gel at 25℃ using a Brookfield DVRT rotational viscometer, and the rotation speed is selected at 20rpm.
[0037] Example 1
[0038] A method for preparing a carbomer resin, specifically, accurately weighing 200g of acrylic acid, 20g of methyl acrylate, 1g of potassium carbonate, 10g of Tween-20, 10g of pentaerythritol diallyl ether, 200g of acetonitrile and 800g of cyclohexane in a four-necked flask, heating to 50°C under nitrogen protection; then adding 10g of azobisisovaleronitrile, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 3000cP, dripping 20g of polyethylene glycol (200) acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (7000cP). At this time, adding 4g of polyethylene glycol (200) acrylate and 0.15g of azobisisovaleronitrile into the reaction system, and continuing to react at this temperature for 2h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product were measured, and the results are shown in Table 1.
[0039] Example 2
[0040] A method for preparing a carbomer resin, specifically, accurately weighing 200g of methacrylic acid, 2g of isooctyl acrylate, 10g of sodium carbonate, 10g of Span-60, 10g of pentaerythritol triallyl ether, 800g of acetic acid and 200g of carbon tetrachloride in a four-necked flask, heating to 90°C under nitrogen protection; then adding 10g of benzoyl peroxide, stirring at a rate of 200rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 2500cP, dropping 10g of polyethylene glycol (1000) acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (6000cP). At this time, adding 4g of polyethylene glycol (1000) acrylate and 0.02g of benzoyl peroxide into the reaction system, and continuing to react at this temperature for 3h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product were measured, and the results are shown in Table 1.
[0041] Example 3
[0042] A method for preparing a carbomer resin comprises the following steps: accurately weighing 100 g of maleic acid, 100 g of crotonic acid, 10 g of stearic acrylate, 10 g of lauryl acrylate, 5 g of sodium chloride, 5 g of calcium chloride, 1 g of Tween-80, 5 g of pentaerythritol triacrylate, 3 g of diallyl phthalate, 300 g of ethyl acetate and 700 g of dichloromethane in a four-necked flask; heating the flask to 65° C. under nitrogen protection; subsequently adding 10 g of azobisisobutyronitrile, stirring at a rate of 300 rpm, reacting at the temperature, using an online viscometer to monitor the viscosity of the system in real time, and dripping 8 g of polyethylene glycol (600) acrylate into the reaction system when the viscosity of the reaction system reaches 3500 cP, and continuing the reaction until the viscosity of the system no longer increases (8000 cP). At this time, 2 g of polyethylene glycol (600) acrylate and 0.07 g of azobisisobutyronitrile were added to the reaction system, and the reaction was continued at the same temperature for 2.5 h. After the reaction was completed, the crude product was washed, filtered, and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product were measured, and the results are shown in Table 1.
[0043] Example 4
[0044] A method for preparing a carbomer resin, specifically, accurately weighing 50g of itaconic acid, 0.25g of stearic acid acrylate, 0.05g of potassium chloride, 0.05g of Span-80, 0.05g of ethylene glycol dimethacrylate, 500g of butyl acetate and 500g of benzene in a four-necked flask, heating to 65°C under nitrogen protection; then adding 0.05g of azobisisoheptanitrile, stirring at a rate of 300rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 2000cP, dropping 0.25g of poly 1,3-propylene glycol (200) acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (5000cP). At this time, adding 0.25g of poly 1,3-propylene glycol (200) acrylate and 0.01g of azobisisoheptanitrile into the reaction system, and continuing to react at this temperature for 1.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0045] Example 5
[0046] A method for preparing a carbomer resin, specifically, accurately weighing 200g of acrylic acid, 20g of acrylic acid palmitate, 10g of sodium bicarbonate, 5g of oleth-10, 5g of hydroxyethyl cellulose, 10g of allyl sucrose ether, 200g of toluene, 200g of tetrahydrofuran and 600g of benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g of dodecyl peroxide and 5g of dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 4000cP, dripping 20g of octanediol acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (10000cP). At this time, adding 3g of octanediol acrylate, 0.05g of dodecyl peroxide and 0.05g of dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0047] Example 6
[0048] A method for preparing a carbomer resin, specifically, accurately weighing 200g of maleic acid, 20g of acrylate palmitate, 10g of sodium bicarbonate, 8g of oleth-10, 10g of allyl sucrose ether, 200g of toluene, 200g of tetrahydrofuran and 600g of benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 2g of dodecyl peroxide and 5g of dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 3000cP, dripping 20g of 12-hydroxylauryl alcohol acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (9000cP). At this time, adding 3g of 12-hydroxylauryl alcohol acrylate, 0.05g of dodecyl peroxide and 0.05g of dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0049] Example 7
[0050] A method for preparing a carbomer resin comprises the following steps: accurately weighing 200 g of acrylic acid, 20 g of acrylate palmitate, 10 g of sodium bicarbonate, 5 g of oleth-10, 5 g of hydroxyethyl cellulose, 10 g of allyl sucrose ether, 200 g of toluene, 200 g of tetrahydrofuran and 600 g of benzene in a four-necked flask, heating the flask to 70°C under nitrogen protection; subsequently adding 5 g of dodecyl peroxide and 5 g of dimethyl azobisisobutyrate, stirring at a rate of 400 rpm, reacting at the temperature, using an online viscometer to monitor the viscosity of the system in real time, and when the viscosity of the reaction system reaches 3500 cP, dripping 12 g of 12-hydroxystearic acid acrylate into the reaction system, and continuing the reaction until the viscosity of the system no longer increases (8500 cP). At this time, 4g 12-hydroxystearic acid acrylate, 0.05g dodecyl peroxide and 0.05g dimethyl azobisisobutyrate were added to the reaction system, and the reaction was continued at the same temperature for 2.5h. After the reaction was completed, the crude product was washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product were measured, and the results are shown in Table 1; Figure 1 The light transmittance comparison of the gels prepared by swelling the carbomer resins prepared in Example 7 and Comparative Example 2 in alcohol substances is shown.
[0051] Example 8
[0052] A method for preparing a carbomer resin comprises the following steps: accurately weighing 200 g of acrylic acid, 20 g of acrylate palmitate, 10 g of sodium bicarbonate, 5 g of oleth-10, 5 g of hydroxyethyl cellulose, 10 g of allyl sucrose ether, 200 g of toluene, 200 g of tetrahydrofuran and 600 g of benzene in a four-necked flask, heating the flask to 70°C under nitrogen protection; subsequently adding 5 g of dodecyl peroxide and 5 g of dimethyl azobisisobutyrate, stirring at a rate of 400 rpm, reacting at the temperature, using an online viscometer to monitor the viscosity of the system in real time, and dripping 12 g of 12-hydroxystearic acid acrylate into the reaction system when the viscosity of the reaction system reaches 4000 cP, and continuing the reaction until the viscosity of the system no longer increases (8500 cP). At this time, 1g of 12-hydroxystearic acid acrylate, 0.01g of dodecyl peroxide and 0.01g of dimethyl azobisisobutyrate were added to the reaction system, and the reaction was continued at this temperature for 2.5h. After the reaction was completed, the crude product was washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product were measured, and the results are shown in Table 1.
[0053] Example 9
[0054] A method for preparing a carbomer resin, specifically, accurately weighing 200g of acrylic acid, 20g of acrylate palmitate, 10g of sodium bicarbonate, 5g of oleth-10, 5g of hydroxyethyl cellulose, 10g of allyl sucrose ether, 200g of toluene, 200g of tetrahydrofuran and 600g of benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g of dodecyl peroxide and 5g of dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 3500cP, dripping 6g of 12-hydroxystearic acid acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (6500cP). At this time, adding 4g of 12-hydroxystearic acid acrylate, 0.05g of dodecyl peroxide and 0.05g of dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0055] Example 10
[0056] A method for preparing a carbomer resin, specifically, accurately weighing 200g of acrylic acid, 20g of acrylate palmitate, 10g of sodium bicarbonate, 5g of oleth-10, 5g of hydroxyethyl cellulose, 10g of allyl sucrose ether, 200g of toluene, 200g of tetrahydrofuran and 600g of benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g of dodecyl peroxide and 5g of dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 3500cP, dripping 12g of 12-hydroxystearic acid acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (8500cP). At this time, adding 4g of octanediol acrylate, 0.05g of dodecyl peroxide and 0.05g of dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0057] Embodiment 11
[0058] A method for preparing a carbomer resin, specifically, accurately weighing 200g of acrylic acid, 20g of acrylic acid palmitate, 10g of sodium bicarbonate, 5g of oleyl alcohol polyether-10, 5g of hydroxyethyl cellulose, 10g of allyl sucrose ether, 200g of toluene, 200g of tetrahydrofuran and 600g of benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 10g of dodecyl peroxide, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 3500cP, dripping 12g of 12-hydroxystearic acid acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (8500cP). At this time, adding 4g of octanediol acrylate and 0.1g of dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product were measured, and the results are shown in Table 1.
[0059] Example 12
[0060] A method for preparing a carbomer resin, specifically, accurately weighing 200g of acrylic acid, 20g of acrylic acid palmitate, 10g of sodium bicarbonate, 5g of oleth-10, 5g of hydroxyethyl cellulose, 10g of allyl sucrose ether, 200g of toluene, 200g of tetrahydrofuran and 600g of benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 10g of dodecyl peroxide, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, when the viscosity of the reaction system reaches 3500cP, dripping 12g of 12-hydroxylauryl alcohol acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (8500cP). At this time, adding 4g of poly 1,3-propylene glycol (200) acrylate and 0.1g of dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product were measured, and the results are shown in Table 1.
[0061] Comparative Example 1
[0062] The preparation of carbomer includes the following steps: accurately weighing 200g acrylic acid, 20g acrylate palmitate, 10g sodium bicarbonate, 5g oleth-10, 5g hydroxyethyl cellulose, 10g allyl sucrose ether, 200g toluene, 200g tetrahydrofuran and 600g benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g dodecyl peroxide and 5g dimethyl azobisisobutyrate, reacting at this temperature for 4 hours, and stirring at a rate of 400rpm. After the reaction is completed, the crude product is washed, filtered and dried. The prepared carbomer product is subjected to alcohol gel transmittance measurement and alcohol gel viscosity measurement, and the results are shown in Table 1.
[0063] Comparative Example 2
[0064] The preparation of carbomer includes the following steps: accurately weigh 200g acrylic acid, 20g acrylate palmitate, 12g 12-hydroxystearic acid acrylate, 10g sodium bicarbonate, 5g oleth-10, 5g hydroxyethyl cellulose, 10g allyl sucrose ether, 200g toluene, 200g tetrahydrofuran and 600g benzene in a four-necked flask, and heat to 70°C under nitrogen protection; then add 5g dodecyl peroxide and 5g dimethyl azobisisobutyrate, react at this temperature for 4 hours, and stir at a rate of 400rpm. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1; Figure 1 It can be seen that the light transmittance of the alcohol gel prepared by the carbomer resin in Example 7 of the present invention is significantly better than that of the alcohol gel prepared by the carbomer resin in Comparative Example 2.
[0065] Comparative Example 3
[0066] The preparation of carbomer includes the following steps: accurately weighing 200g acrylic acid, 20g acrylate palmitate, 10g sodium bicarbonate, 5g oleth-10, 5g hydroxyethyl cellulose, 10g allyl sucrose ether, 200g toluene, 200g tetrahydrofuran and 600g benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g dodecyl peroxide and 5g dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, and when the viscosity of the reaction system reaches 3500cP, 12g 12-hydroxystearic acid acrylate is added dropwise to the reaction system, and the reaction is continued at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The prepared carbomer product is subjected to alcohol gel transmittance measurement and alcohol gel viscosity measurement, and the results are shown in Table 1.
[0067] Comparative Example 4
[0068] The preparation of carbomer comprises the following steps: accurately weighing 200g acrylic acid, 20g acrylate palmitate, 10g sodium bicarbonate, 5g oleth-10, 5g hydroxyethyl cellulose, 10g allyl sucrose ether, 200g toluene, 200g tetrahydrofuran and 600g benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g dodecyl peroxide and 5g dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, and when the viscosity of the reaction system reaches 3500cP, dripping 16g 12-hydroxystearic acid acrylate, 0.05g dodecyl peroxide and 0.05g dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product were measured, and the results are shown in Table 1.
[0069] Comparative Example 5
[0070] The preparation of carbomer comprises the following steps: accurately weighing 200g acrylic acid, 20g acrylate palmitate, 10g sodium bicarbonate, 5g oleth-10, 5g hydroxyethyl cellulose, 10g allyl sucrose ether, 200g toluene, 200g tetrahydrofuran and 600g benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g dodecyl peroxide and 5g dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, and when the viscosity of the reaction system reaches 3500cP, dropping 21g 12-hydroxystearic acid acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (8500cP). At this time, adding 4g 12-hydroxystearic acid acrylate, 0.05g dodecyl peroxide and 0.05g dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0071] Comparative Example 6
[0072] The preparation of carbomer comprises the following steps: accurately weighing 200g acrylic acid, 20g acrylate palmitate, 10g sodium bicarbonate, 5g oleth-10, 5g hydroxyethyl cellulose, 10g allyl sucrose ether, 200g toluene, 200g tetrahydrofuran and 600g benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g dodecyl peroxide and 5g dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, and when the viscosity of the reaction system reaches 3500cP, dropping 12g 12-hydroxystearic acid acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (8500cP). At this time, adding 5g 12-hydroxystearic acid acrylate, 0.05g dodecyl peroxide and 0.05g dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0073] Comparative Example 7
[0074] The preparation of carbomer comprises the following steps: accurately weighing 200g acrylic acid, 20g acrylate palmitate, 10g sodium bicarbonate, 5g oleth-10, 5g hydroxyethyl cellulose, 10g allyl sucrose ether, 200g toluene, 200g tetrahydrofuran and 600g benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g dodecyl peroxide and 5g dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, and when the viscosity of the reaction system reaches 4500cP, dropping 12g 12-hydroxystearic acid acrylate into the reaction system, and continuing to react until the viscosity of the system no longer increases (8500cP). At this time, adding 4g 12-hydroxystearic acid acrylate, 0.05g dodecyl peroxide and 0.05g dimethyl azobisisobutyrate into the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0075] Comparative Example 8
[0076] The preparation of carbomer includes the following steps: accurately weighing 200g acrylic acid, 20g acrylate palmitate, 10g sodium bicarbonate, 5g oleth-10, 5g hydroxyethyl cellulose, 10g allyl sucrose ether, 200g toluene, 200g tetrahydrofuran and 600g benzene in a four-necked flask, heating to 70°C under nitrogen protection; then adding 5g dodecyl peroxide and 5g dimethyl azobisisobutyrate, stirring at a rate of 400rpm, reacting at this temperature, using an online viscometer to monitor the viscosity of the system in real time, and when the viscosity of the reaction system reaches 1500cP, adding 12g 12-hydroxystearic acid acrylate dropwise to the reaction system, and continuing to react until the system viscosity reaches 2500cP. At this time, adding 4g 12-hydroxystearic acid acrylate, 0.05g dodecyl peroxide and 0.05g dimethyl azobisisobutyrate to the reaction system, and continuing to react at this temperature for 2.5h. After the reaction is completed, the crude product is washed, filtered and dried. The alcohol gel transmittance and alcohol gel viscosity of the prepared carbomer product are measured, and the results are shown in Table 1.
[0077] Table 1
[0078]
[0079]
[0080] It can be verified from Examples 1 to 12 that the gel obtained by swelling the Carbomer resin prepared by the technical solution of the present invention in alcoholic substances (taking alcohol as an example) has excellent viscosity and transmittance, with a viscosity greater than 15000 cP and a transmittance greater than 90%, which can meet the needs of high-end daily chemical and pharmaceutical industries. In addition, in combination with Comparative Example 1, it can be verified that the present invention greatly improves the compatibility of the macromolecular chain segment with alcoholic substances by adding α, β-unsaturated acid alcohol ester monomers for copolymerization, so that the viscosity and transmittance of the obtained Carbomer resin alcohol gel can be significantly improved; in combination with Comparative Example 2, it can be verified that the present invention monitors the viscosity of the reaction system in real time, and then adds α, β-unsaturated acid alcohol ester monomers when the viscosity of the reaction system reaches a certain viscosity, so as to avoid the uneven distribution of monomers in the polymer due to the difference in the reactivity rate of each monomer, thereby ensuring that the α, β-unsaturated acid alcohol ester monomers are more evenly distributed in the polymer chain, The viscosity of the gel obtained by swelling the prepared carbomer resin in alcohol substances is thereby increased; in combination with Comparative Examples 3 and 4, it can be further confirmed that the present invention adds α,β-unsaturated acid alcohol ester monomers to the reaction system in batches in a staged addition manner, and adds α,β-unsaturated acid alcohol ester monomers and a second initiator for a second time when the viscosity of the reaction system no longer increases, which can initiate monomer polymerization again on the macromolecular chain that has been polymerized to form a side chain rich in α,β-unsaturated acid polyol ester monomers, thereby accelerating the swelling of the resin in the alcohol solution, and the obtained carbomer resin alcohol gel has better viscosity and light transmittance.
[0081] It should be noted that the above contents are further detailed descriptions of the present invention in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions; the dimensional data of this embodiment does not necessarily limit the technical solution, but only shows one of the specific working conditions. For ordinary technicians in the technical field to which the present invention belongs, several simple improvements and modifications can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A method for preparing a carbomer resin, characterized in that: The method comprises the following steps: in an inert atmosphere, an α,β-unsaturated acid monomer, an α,β-unsaturated acid alkyl ester monomer, a surfactant, a crosslinking agent and a first initiator are subjected to a polymerization reaction in an organic solvent; when the viscosity of the reaction system reaches a first viscosity value, the α,β-unsaturated acid alcohol ester monomer is added to the reaction system for the first time to continue the polymerization reaction; when the viscosity of the reaction system reaches a second viscosity value, a second initiator is added to the reaction system and the α,β-unsaturated acid alcohol ester monomer is added for the second time; after the polymerization reaction is completed, the carbomer resin is obtained; wherein the second viscosity value is greater than the first viscosity value.
2. The method for preparing a carbomer resin according to claim 1, wherein The α,β-unsaturated alcohol ester monomer includes one or more of polyethylene glycol (200) acrylate, polyethylene glycol (600) acrylate, polyethylene glycol (1000) acrylate, polypropylene glycol (200) acrylate, octanediol acrylate, 12-hydroxylauryl alcohol acrylate, and 12-hydroxystearyl alcohol acrylate, and the α,β-unsaturated alcohol ester monomer added for the first time and the α,β-unsaturated alcohol ester monomer added for the second time are of the same or different types; and / or, the mass of the first added α,β-unsaturated acid alcohol ester monomer is 0.5%-10% of the mass of the α,β-unsaturated acid monomer; preferably 2%-8%; And / or, the mass of the α,β-unsaturated acid alcohol ester monomer added for the second time is 0.1%-2% of the mass of the α,β-unsaturated acid monomer; preferably 0.5%-2%.
3. The method for preparing carbomer resin according to claim 1, wherein The first viscosity value is 1000-5000 cP, preferably 2000-4000 cP, and further preferably 2000-3500 cP; And / or, the second viscosity value is the peak viscosity value of the reaction system after the α,β-unsaturated acid alcohol ester monomer is added for the first time.
4. The method for preparing a carbomer resin according to claim 1, wherein The α,β-unsaturated acid monomer includes one or more of acrylic acid, methacrylic acid, maleic acid, crotonic acid and itaconic acid; And / or, the mass of the α,β-unsaturated acid monomer is 5%-20% of the mass of the organic solvent.
5. The method for preparing carbomer resin according to claim 1, characterized in that: The α,β-unsaturated acid alkyl ester monomer includes one or more of methyl acrylate, isooctyl acrylate, stearic acid ester, lauryl acrylate and palmitic acid ester; And / or, the mass of the α,β-unsaturated acid alkyl ester monomer is 0.5%-10% of the mass of the α,β-unsaturated acid monomer.
6. The method for preparing a carbomer resin according to claim 1, wherein The surfactant includes an organic surfactant and an inorganic surfactant, wherein the inorganic surfactant includes one or more of potassium carbonate, sodium carbonate, sodium chloride, potassium chloride, calcium chloride and sodium bicarbonate; the organic surfactant includes one or more of Tween-20, Tween-80, Span-60, Span-80, oleth-10 and hydroxyethyl cellulose; Preferably, the mass of the inorganic surfactant is 0.1%-5% of the mass of the α,β-unsaturated acid monomer; preferably, the mass of the organic surfactant is 0.1%-5% of the mass of the α,β-unsaturated acid monomer.
7. The method for preparing a carbomer resin according to claim 1, wherein The cross-linking agent is a cross-linking agent containing at least two unsaturated carbon-carbon double bonds; Preferably, the cross-linking agent includes one or more of pentaerythritol diallyl ether, pentaerythritol triallyl ether, pentaerythritol triacrylate, diallyl phthalate, ethylene glycol dimethacrylate and allyl sucrose ether; And / or, the mass of the cross-linking agent is 0.1%-5% of the mass of the α,β-unsaturated acid monomer.
8. The method for preparing a carbomer resin according to claim 1, wherein The organic solvent includes a polar organic solvent and a non-polar organic solvent; Preferably, the polar organic solvent comprises one or more of acetonitrile, acetic acid, ethyl acetate, butyl acetate, toluene and tetrahydrofuran; Preferably, the non-polar organic solvent comprises one or more of benzene, cyclohexane, carbon tetrachloride and dichloromethane; And / or, the mass of the polar organic solvent is 20%-80% of the mass of the organic solvent.
9. The method for preparing a carbomer resin according to claim 1, wherein The reaction temperature of the polymerization reaction involved in the preparation method is 50-90°C; And / or, after adding a second initiator and a second addition of the α,β-unsaturated acid alcohol ester monomer to the reaction system, the reaction is stirred for 1-3 hours.
10. The method for preparing a carbomer resin according to claim 1, wherein The first initiator and the second initiator are independently selected from one or more of lauroyl peroxide, benzoyl peroxide, azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanonitrile and dimethyl azobisisobutyrate; and / or, the mass of the first initiator is 0.1%-5% of the mass of the α,β-unsaturated acid monomer; And / or, the mass of the second initiator is 0.1%-5%, preferably 0.5%-4%, and more preferably 0.5%-2.5% of the mass of the α,β-unsaturated alcohol ester monomer added for the second time.
11. A carbomer resin, characterized in that: The carbomer resin is prepared by the method for preparing the carbomer resin according to any one of claims 1 to 10.
Citation Information
Cited By
Method for continuously preparing carbomer resin
CN120737244A