Polyaryletherketone resin with branched structure and preparation method thereof

By introducing the polyaryletherketone resin with a branched structure copolymerized with diphenol, the application limitation of polyetherketone resin in high temperature environments is solved, and the glass transition temperature and mechanics are improved. The performance also reduces the processing temperature window, maintains solvent resistance, and expands its application range.

CN119060324AInactive Publication Date: 2024-12-03山东君昊高性能聚合物有限公司 +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411350314.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The use of a single polyether ether ketone resin in the engineering field is limited by its glass transition temperature and processing properties, and it is difficult to meet the application needs in high temperature environments. At the same time, molecular chain regularity and solvent resistance are easily damaged during the modification process.

Method used

By introducing the isophenyl difluorodione monomer and diphenol, a polyaryletherketone resin with branched structure is formed, which increases the glass transition temperature and reduces the melting point, extends the high-temperature usage time, while retaining good solvent resistance.

Benefits of technology

The mechanical properties of polyether ether ketone resin are improved and the processing temperature window is reduced, the application range in high temperature environment is expanded, and the good solvent resistance is maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060324A_ABST
    Figure CN119060324A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polyether-ether-ketone synthesis, in particular to polyaryletherketone resin with a branched structure and a preparation method thereof.The preparation method comprises the following steps that an m-benzene type difluorodiketone monomer, a diphenol monomer, a first salt-forming agent and a first solvent are placed in a reaction kettle, protective gas is introduced, and under continuous stirring, a reaction is conducted for 1-2 h; carrying out a salt forming reaction at a first reaction temperature, continuously heating to a second reaction temperature to carry out prepolymerization, and finally heating to a third reaction temperature to carry out a polymerization reaction; and after the reaction is finished, performing post-treatment to obtain the polyaryletherketone resin with a branched structure. Compared with conventional polyether-ether-ketone, the polyether-ether-ketone with the branched structure has the advantages that the glass-transition temperature is higher, the mechanical property of the polyether-ether-ketone resin with the structure can be guaranteed due to the large intermolecular acting force, meanwhile, the melting point is lower than that of the conventional polyether-ether-ketone, the processing temperature window is reduced, and the processing cost is reduced. And the resin can be processed at a relatively low melting temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyetheretherketone synthesis, and in particular to a polyaryletherketone resin with a branched structure and a preparation method thereof. Background Art

[0002] Polyetheretherketone is a semi-crystalline aromatic high temperature resistant thermoplastic resin with a high glass transition temperature Tg = 143 ° C, a high melting point Tm = 334 ° C, and a high load heat deformation temperature of 316 ° C. It can be used for a long time at a temperature of 250 ° C and for a short time at a high temperature of 300 ° C. Polyetheretherketone can withstand almost any chemical except concentrated sulfuric acid. Even at high temperatures, it still has good chemical stability.

[0003] At low temperatures, both crystalline and amorphous thermoplastic polymers exhibit a glassy state. When heated in a narrow temperature range, the temperature of the change from the glassy state to a flexible plastic state is called the glass transition temperature (Tg), which represents the temperature at which the molecular chain segments move. When the crystalline polymer continues to be heated, another thermal transition temperature will appear, which is the melting point (Tm). The glass transition temperature and melting point of polymers are usually used as standards for measuring the temperature resistance of polymers. At present, the demand for high-temperature resistant materials is increasing, which has accelerated the research of new high-temperature resistant materials. The performance of a single polyetheretherketone resin is difficult to meet its use requirements in many engineering fields. Therefore, in recent years, the modification of polyetheretherketone resins has never stopped at home and abroad. Through the modification of polyetheretherketone, it can be applied to a wider range of fields.

[0004] Copolymerization by adding phenol in different proportions is an effective method to change the molecular structure, which can improve the processing and molding properties of the product, expand the application range of the product, etc. For example, patent CN200710055849.9 uses fluorinated diphenol and hydroquinone in different proportions to copolymerize to reduce the dielectric constant of polyetheretherketone, but the fluorinated diphenol destroys the regularity of the polyetheretherketone molecular chain, and its solvent resistance is greatly weakened. Summary of the invention

[0005] In order to ensure that the glass transition temperature of polyetheretherketone does not decrease and reduce the temperature window for its processing, a polyaryletherketone resin with a branched structure and a preparation method thereof are provided. The polyetheretherketone with a branched structure of the present invention has a higher glass transition temperature than conventional polyetheretherketone, and the intermolecular force is larger, which can ensure the mechanical properties of the polyetheretherketone resin with the structure. At the same time, the melting point is lower than that of conventional polyetheretherketone, which reduces the temperature window for processing, and the resin can be processed at a lower melting temperature, and the good solvent resistance of polyetheretherketone is also retained.

[0006] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:

[0007] A method for preparing a polyaryletherketone resin having a branched structure comprises the following steps:

[0008] The isophenyl difluorodione monomer, the diphenol monomer, the first salt-forming agent and the first solvent are placed in a reaction kettle, a protective gas is introduced, and a salt-forming reaction is first performed at a first reaction temperature under continuous stirring, the temperature is continuously raised to a second reaction temperature for prepolymerization, and finally the temperature is raised to a third reaction temperature for polymerization reaction;

[0009] After the reaction is completed, post-treatment is performed to obtain a polyaryletherketone resin having a branched structure;

[0010] The chemical structure of the isophthalic difluorodione monomer is as follows:

[0011]

[0012] Furthermore, the isophthalic difluorodiketone monomer is obtained by reacting 4,4'-difluorobenzophenone with resorcinol.

[0013] Furthermore, the specific method for obtaining the isophthalic difluorodione monomer is as follows: 4,4'-difluorobenzophenone, resorcinol, a second salt-forming agent, a water-carrying agent and a second solvent are placed in a reaction kettle, a protective gas is introduced, and toluene gas is released when the water content is consistent with the theoretical value under continuous stirring, and then the temperature is raised to 165-185°C for reaction for 3-8h, and the mother liquor is cooled and filtered to obtain the mother liquor; the mother liquor is stirred to descend, and the product is precipitated with water and a hydrochloric acid solution is added for acidification, the product is filtered out and washed with water until it is neutral, and then the product is purified to obtain the isophthalic difluorodione monomer.

[0014] Preferably, the molar ratio of the 4,4'-difluorobenzophenone, the resorcinol and the second salt-forming agent is 10-12:1:1.55-1.65; the second salt-forming agent is anhydrous sodium carbonate and / or anhydrous potassium carbonate; the water-carrying agent is one of benzene, toluene and xylene, and the amount of the water-carrying agent is 8-15% of the volume of the second solvent; the second solvent is selected from one of N,N-dimethylformamide, N,N-dimethylacetamide, 1-methyl-2-pyrrolidone and dimethyl sulfoxide; the amount of the second solvent is 2-5 times the total weight of the 4,4'-difluorobenzophenone and the resorcinol.

[0015] Preferably, the purification treatment is: dissolving the filtered product by soaking in ethanol at room temperature, washing repeatedly to gradually lighten the color of the monomer, then refluxing the mixture of ethanol and water to remove unreacted impurities such as fluoroketone, and drying at a low temperature below 100°C to obtain the isophthalic difluorodiketone monomer.

[0016] Furthermore, the diphenol monomer is selected from one or more of hydroquinone, biphenol, naphthalene diol, and fluorene diol; the first salt-forming agent is anhydrous sodium carbonate and / or anhydrous potassium carbonate; and the first solvent is selected from diphenyl sulfone.

[0017] Furthermore, the molar ratio of the isophthalic difluorodiketone monomer, the diphenol monomer and the first salt-forming agent is 0.05-0.2:1:1.1-1.15; and the amount of the first solvent used is 4-6 times the total weight of the isophthalic difluorodiketone monomer and the diphenol monomer.

[0018] Furthermore, the first reaction temperature is 160-190°C, and the salt-forming reaction time is 0.5-1.5h; the second reaction temperature is 250-260°C, and the prepolymerization time is 0.5-1.5h; the third reaction temperature is 300-315°C, and the polymerization reaction time is 3-5h.

[0019] Furthermore, the post-treatment is to use water to precipitate the product, crush and dry it after separation, use acetone to reflux 5-6 times until there is no first solvent in the filtrate, wash it with water for many times to remove by-products such as salt, and obtain a polyaryletherketone resin with a branched structure after drying.

[0020] Beneficial technical effects:

[0021] Taking polyetheretherketone as an example, polyaryletherketone has the disadvantages of being difficult to dissolve and requiring harsh processing and molding conditions, and its glass transition temperature is 143°C, which limits its application in certain fields. The present invention aims at the low glass transition temperature of polyetheretherketone. From the perspective of molecular design, a small amount of fluorinated monomers with isophenyl structures are introduced to produce partial branching or light cross-linking structures in the main chain structure of polyetheretherketone. The introduction of partial branching or cross-linking structures can increase the glass transition temperature of polyetheretherketone resin and reduce crystallization performance, thereby increasing the use temperature of polyetheretherketone resin and extending its use time in high temperature environment, which has broad application significance in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the NMR carbon spectrum of isophthalic difluorodione monomer;

[0023] Figure 2 This is the infrared spectrum of isophthalic difluorodione monomer;

[0024] Figure 3 This is the DSC curve of isophthalic difluorodione monomer. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.

[0026] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.

[0027] In addition, it should be noted that the use of terms such as "first" and "second" to limit the reaction temperature is only to facilitate the distinction between the temperatures in each reaction step. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0028] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods.

[0029] The preparation of polyaryletherketone takes polyetheretherketone as an example.

[0030] Example 1

[0031] Isophenylene difluorodione monomer, its chemical structure is as follows:

[0032]

[0033] The specific preparation process includes the following:

[0034] 209.40 g of 4,4'-difluorobenzophenone (0.96 mol), 7.05 g of resorcinol (0.064 mol), 17.69 g of anhydrous potassium carbonate, 46.40 mL of toluene and 464.00 mL of NMP was placed in a reaction kettle, and nitrogen was introduced as a protective gas. The mixture was heated to reflux under continuous stirring. When a small amount of water droplets appeared in the water conveyor, the reflux state was maintained until the amount of water was consistent with the theoretical value, toluene gas was released, and then the temperature was raised to 180°C for reaction for 6 hours. The temperature was then lowered and filtered to remove unreacted salt to obtain a mother liquor. 3000 mL of water was poured into the mother liquor, and a hydrochloric acid solution was added and stirred until the pH of the system was 3-4 (using 30 mL of a hydrochloric acid solution). The mixture was then repeatedly washed with distilled water until it was neutral, and an orange-red granular sample was obtained by suction filtration. After a large amount of ethanol was added and soaked for a period of time, the orange-red granular sample was dissolved, and the excess fluoroketone was removed by repeated washing to become a light yellow powder sample. The remaining fluoroketone was removed by hot reflux with a mixture of ethanol and water (the volume ratio of ethanol to water was 1:1), and the mixture was dried at 100°C to constant weight to obtain a white powder product.

[0035] The product in this case was identified, and its NMR carbon spectrum and infrared spectrum were as follows: Figure 1 , Figure 2 As shown, it can be seen that the product of this structure is indeed obtained; its DSC curve is as follows Figure 3 As shown, it can be seen that the melting point of the isophenyl difluorodione monomer is 115.65°C.

[0036] Example 2

[0037] A method for preparing a polyetheretherketone resin having a branched structure comprises the following steps:

[0038] 25.30 g of isophenyl difluorodione monomer (0.05 mol) of Example 1, 55.05 g of hydroquinone (0.50 mol), 60.01 g of anhydrous sodium carbonate and 425.37 g of diphenyl sulfone were placed in a reaction kettle, nitrogen was introduced as a protective gas, and under continuous stirring, a salt-forming reaction was first carried out at 180° C. for 1 h, and then the temperature was further raised to 260° C. for prepolymerization for 1 h, and finally the temperature was raised to 310° C. for polymerization reaction for 3 h;

[0039] After the reaction is completed, the reaction system is poured into deionized water for precipitation, the precipitate is filtered out, crushed and dried, refluxed with acetone for 5-6 times until there is no diphenyl sulfone in the filtrate, and then washed with deionized water for 5-6 times to remove the solvent and its by-product salt, and dried to obtain a polyaryletherketone resin with a branched structure.

[0040] Example 3

[0041] A method for preparing a polyetheretherketone resin having a branched structure comprises the following steps:

[0042] 12.65 g of isophenyl difluorodione monomer (0.025 mol) of Example 1, 55.05 g of hydroquinone (0.50 mol), 58.29 g of anhydrous sodium carbonate and 395.85 g of diphenyl sulfone were placed in a reaction kettle, nitrogen was introduced as a protective gas, and under continuous stirring, a salt-forming reaction was first carried out at 190° C. for 1 h, and then the temperature was further raised to 250° C. for prepolymerization for 1 h, and finally the temperature was raised to 300° C. for polymerization reaction for 5 h;

[0043] After the reaction is completed, the reaction system is poured into deionized water for precipitation, the precipitate is filtered out, crushed and dried, refluxed with acetone for 5-6 times until there is no diphenyl sulfone in the filtrate, and then washed with deionized water for 5-6 times to remove the solvent and its by-product salt, and dried to obtain a polyaryletherketone resin with a branched structure.

[0044] Example 4

[0045] A method for preparing a polyetheretherketone resin having a branched structure comprises the following steps:

[0046] 37.95 g of isophenyl difluorodione monomer (0.075 mol) of Example 1, 55.05 g of hydroquinone (0.50 mol), 60.94 g of anhydrous sodium carbonate and 454.88 g of diphenyl sulfone were placed in a reaction kettle, nitrogen was introduced as a protective gas, and under continuous stirring, a salt-forming reaction was first carried out at 170° C. for 1 hour, and then the temperature was further raised to 260° C. for prepolymerization for 1 hour, and finally the temperature was raised to 310° C. for polymerization reaction for 4 hours;

[0047] After the reaction is completed, the reaction system is poured into deionized water for precipitation, the precipitate is filtered out, crushed and dried, refluxed with acetone for 5-6 times until there is no diphenyl sulfone in the filtrate, and then washed with deionized water for 5-6 times to remove the solvent and its by-product salt, and dried to obtain a polyaryletherketone resin with a branched structure.

[0048] Comparative Example 1

[0049] In this case, 4,4'-difluorobenzophenone, resorcinol and hydroquinone were used to synthesize the corresponding resin using the synthesis parameters in Example 2. 4,4'-difluorobenzophenone, resorcinol and hydroquinone were configured in a molar ratio of 1.017:0.05:0.5.

[0050] The performance test results of the polyetheretherketone synthesized in each case by the preparation method of the present invention are shown in Table 1.

[0051] Table 1 Properties of polyetheretherketone in each case

[0052]

[0053]

[0054] (Note: The standard sample is conventional polyetheretherketone, which is the polymerization product of hydroquinone and 4,4'-difluorobenzophenone; the chromaticity difference is the chromaticity value of the specific case minus the chromaticity value of the standard sample)

[0055] The glass transition temperature of PEEK in the prior art is 143°C and the melting point is 334°C. However, the polyetheretherketone obtained by the present invention first forms a resorcinol-type difluorodiketone monomer through 4,4'-difluorobenzophenone and resorcinol, and then polymerizes it with hydroquinone to obtain a certain branched structure. Compared with conventional polyetheretherketone, the glass transition temperature is higher, and the intermolecular force is larger, which can ensure the mechanical properties of the polyetheretherketone resin with this structure. At the same time, the melting point is lower than that of conventional polyetheretherketone, which reduces the processing temperature window, and the resin can be processed at a lower melting temperature. In addition, the branched polyetheretherketone of the present invention is black, green and blue in color compared with conventional polyetheretherketone.

[0056] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a polyaryletherketone resin having a branched structure, It is characterized in that The steps include: The isophenyl difluorodione monomer, the diphenol monomer, the first salt-forming agent and the first solvent are placed in a reaction kettle, a protective gas is introduced, and a salt-forming reaction is first performed at a first reaction temperature under continuous stirring, the temperature is continuously raised to a second reaction temperature for prepolymerization, and finally the temperature is raised to a third reaction temperature for polymerization reaction; After the reaction is completed, post-treatment is performed to obtain a polyaryletherketone resin having a branched structure; The chemical structure of the isophthalic difluorodione monomer is as follows:

2. A method for preparing a polyaryletherketone resin having a branched structure according to claim 1, It is characterized in that The isophthalic difluorodione monomer is obtained by reacting 4,4'-difluorobenzophenone with resorcinol.

3. A method for preparing a polyaryletherketone resin having a branched structure according to claim 2, It is characterized in that The specific method for obtaining the isophthalic difluorodione monomer is as follows: 4,4'-difluorobenzophenone, resorcinol, a second salt-forming agent, a water-carrying agent and a second solvent are placed in a reaction kettle, a protective gas is introduced, and toluene gas is released when the water content is consistent with the theoretical value under continuous stirring, and then the temperature is raised to 165-185° C. for reaction for 3-8 hours, and the temperature is lowered and filtered to obtain a mother liquor; the mother liquor is stirred to drop, water is used to precipitate the product, and a hydrochloric acid solution is added to the mother liquor for acidification treatment, and the product is filtered out and washed with water until it is neutral, and then purified to obtain the product isophthalic difluorodione monomer.

4. The method for preparing a polyaryletherketone resin having a branched structure according to claim 3, It is characterized in that The molar ratio of the 4,4'-difluorobenzophenone, the resorcinol, and the second salt-forming agent is 10-12:1:1.55-1.65; The second salt-forming agent is anhydrous sodium carbonate and / or anhydrous potassium carbonate; the water-carrying agent is one of benzene, toluene and xylene, and the amount of the water-carrying agent is 8-15% of the volume of the second solvent; The second solvent is selected from one of N,N-dimethylformamide, N,N-dimethylacetamide, 1-methyl-2-pyrrolidone, and dimethyl sulfoxide; The amount of the second solvent used is 2-5 times the total weight of the 4,4'-difluorobenzophenone and the resorcinol.

5. The method for preparing a polyaryletherketone resin having a branched structure according to claim 3, It is characterized in that The purification treatment is as follows: the filtered product is dissolved by soaking in ethanol at room temperature, washed repeatedly to gradually lighten the color of the monomer, and then refluxed with a mixture of ethanol and water to remove unreacted impurities, and dried at a low temperature below 100° C. to obtain the isophthalic difluorodione monomer.

6. A method for preparing a polyaryletherketone resin having a branched structure according to any one of claims 1 to 5, It is characterized in that The diphenol monomer is selected from one or more of hydroquinone, biphenol, naphthalene diol, and fluorene diol; the first salt-forming agent is anhydrous sodium carbonate and / or anhydrous potassium carbonate; and the first solvent is selected from diphenyl sulfone.

7. A method for preparing a polyaryletherketone resin having a branched structure according to any one of claims 1 to 5, It is characterized in that The molar ratio of the isophthalic difluorodiketone monomer, the diphenol monomer and the first salt-forming agent is 0.05-0.2:1:1.1-1.15; the amount of the first solvent is 4-6 times the total weight of the isophthalic difluorodiketone monomer and the diphenol monomer.

8. A method for preparing a polyaryletherketone resin having a branched structure according to any one of claims 1 to 5, It is characterized in that The first reaction temperature is 160-190° C., and the salt-forming reaction time is 0.5-1.5 h; The second reaction temperature is 250-260°C, and the prepolymerization time is 0.5-1.5h; The third reaction temperature is 300-315° C., and the polymerization reaction time is 3-5 hours.

9. A method for preparing a polyaryletherketone resin having a branched structure according to any one of claims 1 to 5, It is characterized in that The post-treatment is to use water to precipitate the product, crush and dry it after separation, use acetone to reflux for 5-6 times until there is no first solvent in the filtrate, wash it with water for many times, and obtain the polyaryletherketone resin with branched structure after drying.

Citation Information

Patent Citations

  • Preparation method of branching unit-containing polyether-ether-ketone terpolymer

    CN103214638A

  • Industrial synthesis method of high-thermal-stability blocked binphenyl-structure-containing polyaryletherketone resin

    CN104479089A

  • Semi-crystalline biphenyl copolymerized polyether-ether-ketone resin and preparation method thereof

    CN116515101A

  • Improved synthesis method of polyaryletherketone

    CN118344578A

  • Novel controlled crosslinked polyaryletherketone material with improved properties and a process for producing the same

    US20050010015A1