Method for preparing aliphatic carboxylic acid ligand MOF by two-step hydrothermal degradation of waste nylon 66
The waste nylon 66 is degraded and coordinated with metal ions to synthesize the aliphatic carboxylic acid ligand MOF through a two-step hydrothermal method, which solves the problem of high cost of recycling and MOF in waste nylon 66, and realizes high value-added conversion and resource utilization Maximize and suitable for industrial production.
Patent Information
- Application Number
- CN202411226376.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The prior art is difficult to effectively recycle and convert waste nylon 66, and the raw materials cost is high and the environmental pollution is severe during the synthesis of aliphatic carboxylic acid ligand MOF, and there is a lack of simple industrial preparation methods.
Using a two-step hydrothermal method, firstly, the waste nylon 66 and strong alkali compound are hydrolyzed at 180-220°C to obtain a nylon 66 degradation solution, and then coordinate with metal ions to synthesize aliphatic carboxylic acid ligand MOF Materials, simplify process flow and reduce costs.
It realizes the high added value conversion of waste nylon 66, reduces the production cost of MOF, simplifies the production process, is suitable for large-scale industrial production, and promotes resource utilization and environmentally friendly green production.
Smart Images

Figure CN119060355A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of waste polymer degradation and metal-organic framework (MOF) material preparation, and more specifically, relates to a method for preparing aliphatic carboxylic acid ligand MOF by two-step hydrothermal degradation of waste nylon 66, which provides a new low-cost strategy for the synthesis of aliphatic carboxylic acid ligand MOF materials. Background Art
[0002] Nylon is a thermoplastic resin containing repeated amide groups -NHCO- on the main chain of the molecule. It has good mechanical properties, heat resistance, wear resistance, chemical stability and self-lubrication. It can replace metals to meet the requirements of lightweight and cost-reducing downstream industrial products. With the expansion of demand for engineering plastics in areas such as lightweight automobiles in recent years, the use of nylon products has been continuously developed from chemical fibers to engineering plastics, films, and plastic alloys. It has become a typical alternative material for replacing wood, steel, and porcelain with plastics, and the market size has grown steadily year by year. In 2019, the global nylon market size was approximately US$28.15 billion, and it is expected to reach US$47 billion in 2027. However, the widespread use of nylon has also brought about a series of environmental problems. Waste is often discarded in natural environments such as landfills or oceans. Because it is difficult to be biodegraded, the degradation process may take decades or even hundreds of years. Currently, there are very few means for recycling waste nylon. Incineration of waste nylon will produce a large amount of toxic gases such as NO, NO2, and CO. Physical methods have high requirements for raw material purity, and the source of raw materials is limited to unused processing scraps. The quality of recycled products is poor and the added value is low. Chemical recycling degrades waste nylon into monomers for reuse in nylon production. It is a sustainable recycling model. Common recycling technologies include pyrolysis, hydrolysis, alcoholysis, and aminolysis. However, due to the large number of hydrogen bonds between nylon 66 polymer chains, the existing degradation process conditions are harsh, and the product recovery rate is difficult to improve, which seriously limits its recycling and conversion process. Eimontas et al. used copper-impregnated biochar-based catalysts to pyrolyze waste nylon to recover caprolactam and capronitrile (Justas Eimontas, Nerijus Striūgas, Zakarauskas, Ieva Inna Pitak.Metallised seaweed-derived bio-char catalyst preparation and its application in the pyrolysis process forthe waste fishing nets and marine biomass utilisation.Fuel 2024,357,129922); however, the product is a mixture, and the caprolactam content is only 54.3%, and the capronitrile content is 31.7%, the energy consumption is high, and the mixed product separation is difficult. Zhao et al. degraded nylon 66 and then used Brucella to convert it into a polysaccharide flocculant (Haijuan Zhao, Su Sun, Yongming Cui, Muhammad Wajid Ullah, Khulood Fahad Alabbosh, Noureddine Elboughdiri, Jiangang Zhou. Sustainable production of bacterial flocculants by nylon-6,6 microplastics hydrolysate utilizing Brucella intermedia ZL-06. Journal of Hazardous Materials 2024, 465, 133435), but the screening and cultivation cycle of the strain is long, and after the degradation of nylon 66, it is necessary to use organic solution neutralization, vacuum filtration, recrystallization purification and extraction of adipic acid, which is not conducive to large-scale production. At present, there is still a lack of simple methods that can recycle nylon waste on an industrial scale and convert it into high-value products.
[0003] MOF is a type of crystalline compound material with a periodic repeating network structure formed by the self-assembly of metal ions (or metal clusters) and organic ligands through coordination bonds. Its most notable feature is that there are a large number of channels and cavities in the crystal structure, and the porosity can reach more than 90%. This porous structure determines that MOF materials usually have a large specific surface area. In addition, the porosity, pore size, crystallinity and other properties of MOF materials can be customized through synthetic formula adjustment and process control to obtain MOF materials with directional functions. The above characteristics make MOF materials have excellent performance in gas storage, separation and adsorption, electrode materials and battery separators, catalysis, sensing, drug delivery and other fields. At present, the vast majority of MOFs use aromatic carboxylates such as terephthalic acid and 1,3,5-benzenetricarboxylic acid as ligands. MOFs with aliphatic carboxylic acids as ligands occupy a very special position. Aliphatic carboxylic acids are more flexible and give them a unique breathing effect. Moreover, the unique properties of high hydrophobicity, low optical absorption, gas adsorption selectivity and thermal stability make it have unique potential in the fields of photochemistry, photocatalysis, adsorption diffusion, environmental monitoring, etc. However, compared with aromatic carboxylic acid ligand MOF, there are very few types of aliphatic carboxylic acid ligand MOF (for example, MOF with adipic acid as ligand includes Mn, Co, Tb, Zn, Al, UO, Nd, Ca, Zr; there are also some MOFs with aliphatic ligands such as malonic acid, succinic acid, glutaric acid, etc., the types are very limited), and the synthesis process needs to react in an organic solvent system. The synthesis, purification and separation processes all require the use of a large amount of organic solvents, which cause serious pollution to the environment. At present, there is still a lack of industrial preparation methods.
[0004] In the past, the synthesis of MOF usually uses high-purity small molecule monomer raw materials, which have high raw material costs and are not conducive to large-scale production. In recent years, the research on the preparation of MOF by chemically recycling waste plastics has attracted widespread attention. So far, it has been reported that waste polymers such as waste polyethylene terephthalate and polylactic acid are used as precursors to prepare MOF materials (ZL202211401078.5; ZL 202310475738.2; ZL 202310475998.X; ZL 202211401069.6). This has become a novel chemical recycling method that can not only promote waste recycling and solve the pollution problem of waste polymers, but also use low raw material costs to produce high-value MOF products, achieve the goal of maximizing resource utilization, and meet the green, renewable and sustainable green production and circular economy concepts. However, there has been no report on the preparation of aliphatic carboxylic acid ligand MOF using waste nylon 66 as a precursor. Summary of the invention
[0005] In view of the above defects or improvement needs of the prior art, the purpose of the present invention is to provide a method for preparing aliphatic carboxylic acid ligand MOF by two-step hydrothermal degradation of waste nylon 66, wherein the overall process design of the method is improved, and a high value-added MOF product is prepared from waste nylon 66 raw materials through a two-step hydrothermal method. The present invention utilizes the first step hydrothermal reaction to degrade nylon 66 into adipic acid salt and hexamethylenediamine, and utilizes the second step hydrothermal reaction to directly coordinate the degradation liquid with metal ions to prepare aliphatic carboxylic acid ligand MOF materials. The present invention upgrades chemical recycling of waste nylon 66 and directly uses it as a precursor liquid to synthesize aliphatic carboxylic acid ligand MOFs of various morphologies. The method is simple, realizes waste resource utilization, improves resource utilization, reduces MOF production costs, and simplifies the production process, which is suitable for industrial-scale production of MOF.
[0006] To achieve the above object, the present invention provides a method for preparing aliphatic carboxylic acid ligand MOF by two-step hydrothermal degradation of waste nylon 66, characterized in that it comprises the following steps:
[0007] S1. Dispersing waste nylon 66 and a strong base compound in water to obtain a dispersion; wherein the mass ratio of the strong base compound to the waste nylon 66 is 0.17 to 0.4:1;
[0008] S2. The dispersion obtained in step S1 is subjected to a hydrothermal reaction at 180 to 220° C. for 12 to 48 hours to hydrolyze nylon 66 to obtain a nylon 66 degradation liquid;
[0009] S3. Add a metal salt solution to the nylon 66 degradation liquid obtained in step S2, and continue the hydrothermal reaction at 60-160° C. for 3-24 hours to coordinate the adipate and hexamethylenediamine in the degradation liquid with the metal ions to synthesize MOF. The obtained product is an aliphatic carboxylic acid ligand MOF material; wherein the metal element in the MOF material is the same as the metal element in the metal salt solution.
[0010] As a further preferred embodiment of the present invention, in step S1, the strong base compound is at least one of sodium hydroxide and potassium hydroxide.
[0011] As a further preferred embodiment of the present invention, in step S3, the metal salt in the metal salt solution is at least one of cobalt nitrate, bismuth nitrate, terbium nitrate, europium chloride, lanthanum nitrate and cadmium nitrate.
[0012] As a further preferred embodiment of the present invention, the ratio of the metal salt contained in the metal salt solution in step S3 to the waste nylon 66 in step S1 satisfies a mass ratio of 0.6 to 2.5:1.
[0013] Through the above technical scheme conceived by the present invention, compared with the prior art, in the method of the present invention, the first step of the hydrothermal reaction is to hydrolyze nylon 66 to degrade it and obtain a nylon 66 degradation liquid, which is a degradation reaction; the second step of the hydrothermal reaction is to directly coordinate the nylon 66 degradation liquid with metal ions to prepare aliphatic carboxylic acid ligand MOF materials, which is a coordination reaction. In the first step of the hydrothermal reaction, the hydroxyl ion of the strong base compound is used to break the amide bond to achieve the degradation of nylon 66. The obtained nylon 66 degradation liquid is weakly alkaline, which is not only conducive to ensuring the purity and stability of the degradation product and reducing the occurrence of side reactions, but also can effectively reduce the loss of equipment and further ensure the safety of the reaction. The nylon 66 degradation liquid obtained by the first step of the hydrothermal reaction of the present invention is directly used as a precursor for MOF synthesis, without further purification, and without adding acid to adjust the pH, which simplifies the cumbersome steps of polyamide recycling and can maximize the utilization rate of raw materials. The weakly alkaline degradation solution provides a mild reaction environment, which can promote the coordination reaction of adipate and hexamethylenediamine with metal ions and reduce the occurrence of side reactions. Adipate has a high solubility and can be evenly distributed in the aqueous solution, improving the reaction efficiency and product uniformity. At the same time, the amino group of hexamethylenediamine will not be protonated. Its long chain structure and flexibility enable the molecule to adapt to different coordination requirements in three-dimensional space, and work together with adipate to synthesize MOF materials with different pore sizes, morphologies and functions. Metal ions and organic ligands self-assemble through coordination bonds to gradually form highly ordered MOF crystals.
[0014] Specifically, the present invention can achieve the following beneficial effects:
[0015] (1) Compared with the traditional method of synthesizing MOF, which usually requires de novo synthesis or purchase of purified small molecule organic ligands, the present invention uses waste nylon as raw material, and the adipate in its degradation liquid can be used as an organic ligand for MOF synthesis. Using waste plastics as raw materials for the production of high-value products can reduce the production cost of MOF, promote the recycling of waste plastics, solve the pollution problem of waste plastics, and realize waste resource utilization.
[0016] (2) The existing chemical recovery methods, such as thermally decomposing nylon with a catalyst into a mixed product such as caprolactam and capronitrile, or converting it into a flocculant, etc., all require complex separation and purification steps for the degradation products of nylon before product recovery can be achieved. The present invention does not require separation and purification of hexamethylenediamine and adipic acid products from the degradation liquid after nylon degradation, thus reducing the process and related equipment investment in chemical production, simplifying the production process, thereby reducing production costs and improving production efficiency.
[0017] (3) The method of the present invention prepares aliphatic carboxylic acid ligand MOF by two-step hydrothermal degradation of waste nylon 66, wherein the first hydrothermal reaction is to degrade nylon 66, and the hydrothermal reaction needs to be carried out at 180-220°C for 12-48 hours to ensure sufficient degradation of nylon 66; the second hydrothermal reaction is to directly coordinate the nylon 66 degradation liquid with metal ions to prepare aliphatic carboxylic acid ligand MOF material, and the hydrothermal reaction needs to be continued at 60-160°C for 3-24 hours to avoid excessive temperature affecting the synthesis of the target MOF material.
[0018] In summary, the present invention realizes the high added value transformation of waste plastics through the method of preparing aliphatic carboxylic acid ligand MOF by two-step hydrothermal degradation of waste nylon 66. The proposed method of recycling waste nylon can solve the pollution problem of waste polymers. High-value MOF products can be produced through a simple process flow with low raw material costs, achieving the goal of maximizing resource utilization, realizing cost reduction and efficiency improvement in large-scale production, and also conforming to the green, renewable and sustainable green production and circular economy concepts. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The X-ray powder diffraction spectrum and scanning electron microscope image of the Co-MOF material prepared in Example 1.
[0020] in, Figure 1 a in the equation corresponds to the X-ray powder diffraction spectrum. Figure 1 b in FIG. 1 corresponds to a scanning electron micrograph.
[0021] Figure 2 The X-ray powder diffraction spectrum and scanning electron microscope image of the Bi-MOF material prepared in Example 2.
[0022] in, Figure 2 a in the equation corresponds to the X-ray powder diffraction spectrum. Figure 2 b in FIG. 1 corresponds to a scanning electron micrograph.
[0023] Figure 3 These are the X-ray powder diffraction spectrum and scanning electron microscope image of the Tb-MOF material prepared in Example 3.
[0024] in, Figure 3 a in the equation corresponds to the X-ray powder diffraction spectrum. Figure 3 b in FIG. 1 corresponds to a scanning electron micrograph.
[0025] Figure 4 X-ray powder diffraction spectrum and scanning electron microscope image of the Eu-MOF material prepared in Example 4.
[0026] in, Figure 4 a in the equation corresponds to the X-ray powder diffraction spectrum. Figure 4 b in FIG. 1 corresponds to a scanning electron micrograph.
[0027] Figure 5 These are the X-ray powder diffraction spectrum and scanning electron microscope image of the La-MOF material prepared in Example 5.
[0028] in, Figure 5 a in the equation corresponds to the X-ray powder diffraction spectrum. Figure 5 b in FIG. 1 corresponds to a scanning electron micrograph.
[0029] Figure 6 These are the X-ray powder diffraction spectrum and scanning electron microscope image of the Cd-MOF material prepared in Example 6.
[0030] in, Figure 6 a in the equation corresponds to the X-ray powder diffraction spectrum. Figure 6 b in FIG. 1 corresponds to a scanning electron micrograph.
[0031] Figure 7 This is the X-ray powder diffraction spectrum of the material prepared in Comparative Example 1.
[0032] Figure 8 This is the X-ray powder diffraction spectrum of the material prepared in Comparative Example 2. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0034] In general, the method of the present invention is to add nylon 66 and a strong base compound into a reactor, add water to dissolve the strong base compound, then seal the solution in the reactor, react at 180-220°C, then add a metal salt solution, and react at 60-160°C to obtain an aliphatic carboxylic acid ligand MOF material.
[0035] The following are specific embodiments:
[0036] Example 1
[0037] Weigh 3.0g of waste nylon 66 and 0.7g of potassium hydroxide into a reactor, add 30mL of deionized water, seal the reactor and put it into an oven, heat it at 160°C for 18h, then dissolve 4.27g of cobalt nitrate hexahydrate in 30mL of deionized water, add it to the reactor and seal it again, continue the reaction at 60°C for 20h, wash and dry the product to obtain Co-MOF material with a yield of 85%.
[0038] Figure 1 a in the figure is the X-ray powder diffraction spectrum of Co-MOF material. Figure 1 b is a scanning electron microscope image of the Co-MOF material. From the X-ray powder diffraction spectrum, it can be seen that the Co-MOF material has significant characteristic diffraction peaks, indicating that Co-MOF was successfully synthesized and has good crystallinity. From the scanning electron microscope image, it can be seen that the morphology of the Co-MOF material is stacked flake crystals of 5 to 10 μm.
[0039] Example 2
[0040] Weigh 1.5g of waste nylon 66 and 0.45g of sodium hydroxide into a reactor, add 30mL of deionized water, seal the reactor and put it into an oven, heat it at 180°C for 24h, then dissolve 2.78g of bismuth nitrate pentahydrate in 30mL of deionized water, add it to the reactor and seal it again, continue the reaction at 120°C for 12h, wash and dry the product to obtain Bi-MOF material with a yield of 88%.
[0041] Figure 2 a in the figure is the X-ray powder diffraction spectrum of Bi-MOF material. Figure 2 b is a scanning electron microscope image of the Bi-MOF material. From the X-ray powder diffraction spectrum, it can be seen that the Bi-MOF material has significant characteristic diffraction peaks, indicating that Bi-MOF has been successfully synthesized and has good crystallinity. From the scanning electron microscope image, it can be seen that the morphology of the Bi-MOF material is stacked nanosheets of 150 to 300 nm.
[0042] Example 3
[0043] Weigh 1.0g of waste nylon 66 and 0.25g of sodium hydroxide into a reactor, add 30mL of deionized water, seal the reactor and put it into an oven, heat it at 220°C for 12h, then dissolve 2.47g of terbium nitrate hexahydrate in 30mL of deionized water, add it to the reactor and seal it again, continue the reaction at 90°C for 5h, wash and dry the product to obtain Tb-MOF material with a yield of 93%.
[0044] Figure 3 a in the figure is the X-ray powder diffraction spectrum of Tb-MOF material. Figure 3b in the figure is a scanning electron microscope image of the Tb-MOF material. From the X-ray powder diffraction spectrum, it can be seen that the Tb-MOF material has significant characteristic diffraction peaks, indicating that Tb-MOF has been successfully synthesized and has good crystallinity. From the scanning electron microscope image, it can be seen that the morphology of the Tb-MOF material is stacked flake crystals of 15 to 30 μm.
[0045] Example 4
[0046] Weigh 1.5g of waste nylon 66 and 0.5g of potassium hydroxide into a reactor, add 30mL of deionized water, seal the reactor and put it into an oven, heat it at 200°C for 24h, then dissolve 3.12g of europium chloride hexahydrate in 30mL of deionized water, add it to the reactor and seal it again, continue the reaction at 160°C for 3h, wash and dry the product to obtain Eu-MOF material with a yield of 98%.
[0047] Figure 4 a in the figure is the X-ray powder diffraction spectrum of Eu-MOF material. Figure 4 Figure b is a scanning electron microscope image of the Eu-MOF material. From the X-ray powder diffraction spectrum, it can be seen that the Eu-MOF material has significant characteristic diffraction peaks, indicating that Eu-MOF has been successfully synthesized and has good crystallinity. From the scanning electron microscope image, it can be seen that the morphology of the Eu-MOF material is stacked flake crystals of 2 to 2.5 μm.
[0048] Example 5
[0049] Weigh 2.0g of waste nylon 66 and 0.8g of sodium hydroxide into a reactor, add 30mL of deionized water, seal the reactor and put it into an oven, heat it at 160°C for 36h, then dissolve 1.33g of lanthanum nitrate hexahydrate in 30mL of deionized water, add it to the reactor and seal it again, continue the reaction at 90°C for 10h, wash and dry the product to obtain La-MOF material with a yield of 97%.
[0050] Figure 5 a in the figure is the X-ray powder diffraction spectrum of La-MOF material. Figure 5 b is a scanning electron microscope image of La-MOF material. From the X-ray powder diffraction spectrum, it can be seen that La-MOF material has significant characteristic diffraction peaks, indicating that La-MOF has been successfully synthesized and has good crystallinity. From the scanning electron microscope image, it can be seen that the morphology of La-MOF material is 0.5-1μm slender rod-shaped crystals.
[0051] Example 6
[0052] Weigh 2.5g of waste nylon 66 and 0.4g of sodium hydroxide into a reactor, add 30mL of deionized water, seal the reactor and put it into an oven, heat it at 200°C for 18h, then dissolve 4.31g of cadmium nitrate tetrahydrate in 30mL of deionized water, add it to the reactor and seal it again, continue the reaction at 100°C for 24h, wash and dry the product to obtain Cd-MOF material with a yield of 99%.
[0053] Figure 6 a in the figure is the X-ray powder diffraction spectrum of Cd-MOF material. Figure 6 Figure b is a scanning electron microscope image of the Cd-MOF material. From the X-ray powder diffraction spectrum, it can be seen that the Cd-MOF material has significant characteristic diffraction peaks, indicating that Cd-MOF has been successfully synthesized and has good crystallinity. From the scanning electron microscope image, it can be seen that the Cd-MOF material is a stacked sheet crystal with a size of 400 to 700 nm.
[0054] Comparative Example 1
[0055] Weigh 3.0g of waste nylon 66 and 0.7g of potassium hydroxide into a reactor, add 30mL of deionized water, seal the reactor and put it into an oven, heat it at 120°C for 12h, then dissolve 4.27g of cobalt nitrate hexahydrate in 30mL of deionized water, add it into the reactor and seal it again, continue the reaction at 60°C for 20h, wash and dry the product, and its X-ray powder diffraction spectrum is as follows Figure 7 As shown, the analysis showed that it was a mixture of nylon and Co(OH)2. It can be seen that the first step hydrothermal reaction failed to degrade nylon 66.
[0056] Comparative Example 2
[0057] Weigh 1.0g of waste nylon 66 and 0.25g of sodium hydroxide into a reactor, add 30mL of deionized water, seal the reactor and put it into an oven, heat it at 220°C for 12h, then dissolve 2.47g of terbium nitrate hexahydrate in 30mL of deionized water, add it into the reactor and seal it again, continue the reaction at 200°C for 24h, wash and dry the product, and its X-ray powder diffraction spectrum is as follows: Figure 8 As shown, no obvious characteristic diffraction peaks appear, indicating that too high a reaction temperature during the second step coordination reaction (ie, the second step hydrothermal reaction) is not conducive to the synthesis of MOF.
[0058] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing aliphatic carboxylic acid ligand MOF by two-step hydrothermal degradation of waste nylon 66, characterized in that: The following steps are involved: S1. Dispersing waste nylon 66 and a strong base compound in water to obtain a dispersion; wherein the mass ratio of the strong base compound to the waste nylon 66 is 0.17 to 0.4:1; S2. The dispersion obtained in step S1 is subjected to a hydrothermal reaction at 180 to 220° C. for 12 to 48 hours to hydrolyze nylon 66 to obtain a nylon 66 degradation liquid; S3. Add a metal salt solution to the nylon 66 degradation liquid obtained in step S2, and continue the hydrothermal reaction at 60-160° C. for 3-24 hours to coordinate the adipate and hexamethylenediamine in the degradation liquid with the metal ions to synthesize MOF. The obtained product is an aliphatic carboxylic acid ligand MOF material; wherein the metal element in the MOF material is the same as the metal element in the metal salt solution.
2. The method according to claim 1, characterized in that: In step S1, the strong base compound is at least one of sodium hydroxide and potassium hydroxide.
3. The method according to claim 1, characterized in that: In step S3, the metal salt in the metal salt solution is at least one of cobalt nitrate, bismuth nitrate, terbium nitrate, europium chloride, lanthanum nitrate, and cadmium nitrate.
4. The method according to claim 1, characterized in that: The ratio of the metal salt contained in the metal salt solution in step S3 to the waste nylon 66 in step S1 satisfies a mass ratio of 0.6 to 2.5:1.
Citation Information
Patent Citations
Mechano-chemical method for preparing metal-organic framework material
CN115678030A
Method for preparing metal-organic framework by degrading polyimide through solvothermal
CN117229515A
Production method with reclaimed waste nylon as material
CN1569802A
NANO particle / polyamide composite material, preparation method therefor, and use thereof
US20140048738A1
Cited By
Modified polyester resin for powder coating and preparation method thereof
CN120699518A